Preparation method of high-purity aluminum oxide

By treating dilute sulfuric acid, sodium hydroxide and aluminum chloride of industrial aluminum hydroxide, impurities are removed and calcined, high-purity aluminum oxide is obtained, which solves the problems of complex process, serious pollution and high energy consumption in the existing technology, and achieves the High purity and industrial production goals.

CN119038588APending Publication Date: 2024-11-29XIHUA UNIV +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411143136.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing high-purity alumina production methods have complex processes, serious pollution, high energy consumption, high safety hazards and high requirements for raw material purity, making it difficult to achieve simplified industrial production.

Method used

By gradually treating industrial aluminum hydroxide with dilute sulfuric acid, sodium hydroxide and aluminum chloride solutions, precipitation and washing, removing impurities of sodium, iron and silicon, calcining to obtain high-purity aluminum oxide, and using the recycling of sodium hydroxide to reduce energy Consumption.

Benefits of technology

The preparation of high-purity alumina is achieved, with simplified process, pollution-free, low alkali consumption, and easy to industrial production. The product purity is higher than 99.9 wt%, and the particle size is uniform.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation method of high-purity aluminum oxide, which comprises the following steps: adding dilute sulphuric acid into industrial aluminum hydroxide containing sodium, iron and silicon impurities to form an aluminum sulfate solution, and removing the silicon impurities; adding a sodium hydroxide solution to remove iron impurities; and finally, adding an aluminum chloride solution to form a precipitate, removing sodium impurities, and washing, drying and calcining the precipitate to obtain the high-purity aluminum oxide. The reaction process is easy to operate, the technological process is simplified, no toxic reagent is involved in the preparation process, pollution is avoided, alkali consumption is low, industrialization is facilitated, the purity of the prepared aluminum oxide is higher than 99.9 wt%, the particle size is uniform, and powder is superfine; the intermediate product sodium hydroxide can be recycled, continuous production is realized, and energy consumption is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of inorganic non-metallic materials, and specifically relates to a method for preparing high-purity aluminum oxide. Background Art

[0002] Alumina (Al2O3) structural ceramics have the advantages of high temperature resistance, wear resistance, small linear expansion coefficient, good thermal stability, high hardness, small dielectric constant, large volume resistivity and low price. It is an important basic material indispensable for national economic construction and national defense equipment. The raw materials for the production of alumina in the existing technology are mainly industrial alumina. Although the above industrial raw materials are widely available, they usually contain metal impurities such as sodium and iron. Studies have shown that the higher the mass fraction of impurities, the worse the thermal conductivity, insulation and compressive strength of the material and its products. High-purity alumina powder has optical, electrical, magnetic, thermal and mechanical properties that ordinary alumina powder cannot match, and is widely used in the field of high-tech new materials and modern industry. With the inclusion of core devices such as phase shifters, T / R components, and high-power phased array radars above the X-band in the national key special projects, the demand for high-purity Al2O3 has increased significantly.

[0003] The aluminum sulfate ammonia method, Bayer method, high-purity aluminum powder hydrolysis method and alcohol aluminum method are commonly used methods for producing high-purity alumina. The Bayer method is more difficult to process bauxite with a low aluminum-silicon ratio, and the purity of the resulting alumina depends largely on the quality of the aluminum hydroxide seed crystals. The aluminum sulfate ammonia method has a long production cycle, and the production of NH3 and SO3 during the preparation process will cause serious pollution to the environment, and exhaust gas treatment must be strictly carried out. Both the aluminum powder hydrolysis method and the alcohol aluminum method have high requirements for the purity of the raw material elemental aluminum, and the temperature, pressure and time must be strictly controlled, and the process flow is complicated. The aluminum powder hydrolysis method produces hydrogen during the preparation process, which can easily cause an explosion, and the safety hazards are difficult to eliminate. The alcohol aluminum method requires the use of expensive organic alcohol reagents, and it is necessary to find a suitable catalyst to promote the chemical reaction between aluminum and alcohol, and the product conversion rate and crystallinity are low.

[0004] Therefore, a high-purity alumina and a preparation method thereof with a simple preparation process, which uses raw materials that can be industrially produced and has low energy consumption is urgently needed in the industry. Summary of the invention

[0005] In view of the above shortcomings, the purpose of the present invention is to provide a method for preparing high-purity aluminum oxide. The method is directed to industrial aluminum hydroxide containing sodium, iron, and silicon impurities, and dilute sulfuric acid is added to form an aluminum sulfate solution to remove silicon impurities; then a sodium hydroxide solution is added to remove iron impurities; finally, an aluminum chloride solution is added to form a precipitate to remove sodium impurities, and the precipitate is washed, dried, and calcined to obtain high-purity aluminum oxide. While obtaining high-purity aluminum oxide, the method can simplify the process flow, be pollution-free, and be easy to industrialize, and the intermediate product sodium hydroxide can be recycled to achieve continuous production and reduce energy consumption, and the purity of the obtained aluminum oxide is higher than 99.9wt%.

[0006] The present invention is achieved by the following technical means:

[0007] The invention discloses a method for preparing high-purity aluminum oxide, comprising:

[0008] (1) At room temperature, according to the mass of industrial aluminum hydroxide, 30wt% dilute sulfuric acid of 1-2 times the theoretical molar content of aluminum is added, and the mixture is heated at 70-90°C and stirred for 40-60 minutes in a magnetic stirrer to precipitate silicate ions in the aluminum hydroxide powder into silicic acid, and the precipitate in the solution is filtered to obtain an aluminum sulfate solution.

[0009] (2) Take the aluminum sulfate solution after the above reaction is completely filtered, add sodium hydroxide solution at room temperature, adjust the pH value to between 12 and 14, stir and react for 5 to 10 minutes to completely precipitate the iron ions, and after the reaction is complete, filter the solution. The aluminum sulfate solution reacts to generate a sodium aluminate solution.

[0010] (3) Take the above sodium aluminate solution, add aluminum chloride solution with a theoretical molar content of 1-1.5 times of aluminum, so that aluminum ions are precipitated as white aluminum hydroxide precipitates, and the filtered precipitates are washed with 20-100° C. ultrapure water for multiple times, and dried to obtain high-purity aluminum oxide precursor aluminum hydroxide, and the aluminum hydroxide is calcined to obtain high-purity aluminum oxide. The precipitation washing end point is detected with a silver nitrate solution, and the chloride ions and silver ions react to form a white precipitate. If a white precipitate appears, it means that the chloride ions in the precursor have not been washed out, and the washing should be continued until the white precipitate cannot be detected with silver nitrate.

[0011] The beneficial effects of the present invention are:

[0012] 1. The present invention effectively removes iron, silicon and sodium impurities.

[0013] 2. The reaction process of the present invention is simple to operate, the process flow is simplified, the preparation process does not involve toxic reagents and is pollution-free, the alkali consumption is low, and it is easy to industrialize.

[0014] 3. The aluminum oxide prepared by the present invention is an ultrafine powder with a purity higher than 99.9wt% and uniform particle size. DETAILED DESCRIPTION

[0015] In order to explain the present invention more clearly, the present invention is further described below in conjunction with embodiments. It should be understood by those skilled in the art that the content specifically described below is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.

[0016] Embodiment 1:

[0017] Add 30wt% sulfuric acid with 1.5 times the theoretical molar content of aluminum to 0.2mol of industrial aluminum hydroxide powder, set the temperature to 70°C in a magnetic stirrer, and heat for 40min to generate an aluminum sulfate solution, filter out impurities that cannot be dissolved and react to form silicic acid, add 30wt% sodium hydroxide solution to the filtered aluminum sulfate solution, set the pH value to 13, and form a sodium aluminate solution. Filter out impurities in the sodium aluminate solution, add an aluminum chloride solution with 1 times the theoretical molar content of sodium aluminate to the filtered sodium aluminate solution, and obtain an aluminum hydroxide precipitate, and continuously wash the aluminum hydroxide precipitate with 20°C ultrapure water until there is no white precipitate when a silver nitrate solution is dropped into the filtrate, to obtain a precursor aluminum hydroxide, and calcine the dried precursor to obtain a high-purity aluminum oxide powder.

[0018] Embodiment 2:

[0019] Add 30wt% sulfuric acid with 1.5 times the theoretical molar content of aluminum to 0.2mol of industrial aluminum hydroxide powder, set the temperature to 70°C in a magnetic stirrer, and generate an aluminum sulfate solution after heating for 40min. Filter out impurities that cannot be dissolved and react to form silicic acid, add 30wt% sodium hydroxide solution to the filtered aluminum sulfate solution, set the pH value to 14, and form a sodium aluminate solution. Filter out impurities in the sodium aluminate solution, add an aluminum chloride solution with 1 times the theoretical molar content of sodium aluminate to the filtered sodium aluminate solution, and obtain an aluminum hydroxide precipitate. The aluminum hydroxide precipitate is continuously washed with 20°C ultrapure water until there is no white precipitate when a silver nitrate solution is dripped into the filtrate to obtain a precursor aluminum hydroxide, and the dried precursor is calcined to obtain a high-purity aluminum oxide powder.

[0020] Embodiment 3:

[0021] Add 30wt% sulfuric acid with 1.5 times the theoretical molar content of aluminum to 0.2mol of industrial aluminum hydroxide powder, set the temperature to 70°C in a magnetic stirrer, and react to generate an aluminum sulfate solution after heating for 40min, filter out impurities that cannot be dissolved and react to form silicic acid, add 30wt% sodium hydroxide solution to the filtered aluminum sulfate solution, adjust the pH value to 12, and form a sodium aluminate solution. Filter out impurities in the sodium aluminate solution, add an aluminum chloride solution with 1 times the theoretical molar content of sodium aluminate to the filtered sodium aluminate solution, and obtain an aluminum hydroxide precipitate, and continuously wash the aluminum hydroxide precipitate with 20°C ultrapure water until there is no white precipitate when a silver nitrate solution is dropped into the filtrate, to obtain a precursor aluminum hydroxide, and calcine the dried precursor to obtain a high-purity aluminum oxide powder.

[0022] Embodiment 4:

[0023] Add 30wt% sulfuric acid with 1.5 times the theoretical molar content of aluminum to 0.2mol of industrial aluminum hydroxide powder, set the temperature to 70°C in a magnetic stirrer, generate an aluminum sulfate solution after heating for 60min, filter out impurities that cannot be dissolved and react to form silicic acid, add 30wt% sodium hydroxide solution to the filtered aluminum sulfate solution, adjust the pH value to 12, and form a sodium aluminate solution. Filter out impurities in the sodium aluminate solution, add aluminum chloride solution with 1.5 times the theoretical molar content of sodium aluminate to the filtered sodium aluminate solution, and obtain aluminum hydroxide precipitate, and continuously wash the aluminum hydroxide precipitate with 20°C ultrapure water until no white precipitate is produced by dripping silver nitrate solution into the filtrate, and obtain a precursor aluminum hydroxide, and calcine the dried precursor to obtain a high-purity aluminum oxide powder.

[0024] Embodiment 5:

[0025] Add 30wt% sulfuric acid with 1.5 times the theoretical molar content of aluminum to 0.2mol of industrial aluminum hydroxide powder, set the temperature to 90°C in a magnetic stirrer, generate an aluminum sulfate solution after heating for 60min, filter out impurities that cannot be dissolved and react to form silicic acid, add 30wt% sodium hydroxide solution to the filtered aluminum sulfate solution, adjust the pH value to 12, and form a sodium aluminate solution. Filter out impurities in the sodium aluminate solution, add aluminum chloride solution with 1.5 times the theoretical molar content of sodium aluminate to the filtered sodium aluminate solution, and obtain aluminum hydroxide precipitate, and continuously wash the aluminum hydroxide precipitate with 20°C ultrapure water until no white precipitate is produced by dripping silver nitrate solution into the filtrate, and obtain a precursor aluminum hydroxide, and calcine the dried precursor to obtain a high-purity aluminum oxide powder.

[0026] Embodiment 6:

[0027] 30wt% sulfuric acid with 1.5 times the theoretical molar content of aluminum is added to 0.2mol of industrial aluminum hydroxide powder, the temperature is set to 70°C in a magnetic stirrer, and an aluminum sulfate solution is generated after heating for 60min, and impurities that cannot be dissolved and react to form silicic acid are filtered out, and a 30wt% sodium hydroxide solution is added to the filtered aluminum sulfate solution, and the pH value is adjusted to 12 to form a sodium aluminate solution. Impurities in the sodium aluminate solution are filtered out, and an aluminum chloride solution with 1.5 times the theoretical molar content of sodium aluminate is added to the filtered sodium aluminate solution to obtain an aluminum hydroxide precipitate, and the aluminum hydroxide precipitate is continuously washed with ultrapure water heated to 70°C until there is no white precipitate when a silver nitrate solution is dropped into the filtrate to obtain a precursor aluminum hydroxide, and the precipitate is ultrasonically dispersed, and the dried precursor is calcined to obtain a high-purity aluminum oxide powder.

[0028] Embodiment 7:

[0029] 30wt% sulfuric acid with 1.5 times the theoretical molar content of aluminum is added to 0.2mol of industrial aluminum hydroxide powder, the temperature is set to 70°C in a magnetic stirrer, and an aluminum sulfate solution is generated after heating for 60min, and impurities that cannot be dissolved and react to form silicic acid are filtered out, and 30wt% sodium hydroxide solution is added to the filtered aluminum sulfate solution, and the pH value is adjusted to 12 to form a sodium aluminate solution. Impurities in the sodium aluminate solution are filtered out, and an aluminum chloride solution with 1.5 times the theoretical molar content of sodium aluminate is added to the filtered sodium aluminate solution to obtain an aluminum hydroxide precipitate, and the aluminum hydroxide precipitate is continuously washed with ultrapure water heated to 90°C until there is no white precipitate when a silver nitrate solution is dropped into the filtrate to obtain a precursor aluminum hydroxide, and the precipitate is ultrasonically dispersed, and the dried precursor is calcined to obtain a high-purity aluminum oxide powder.

[0030] Comparative Example 1:

[0031] Add 30wt% sulfuric acid with 1 times the theoretical molar content of aluminum to 0.2mol of industrial aluminum hydroxide powder, stir in a magnetic stirrer for 40min to generate an aluminum sulfate solution, filter out impurities that cannot be dissolved and react to form silicic acid, add 30wt% sodium hydroxide solution to the filtered aluminum sulfate solution, set the pH to 12, and form a sodium aluminate solution. Filter out impurities in the sodium aluminate solution, add aluminum chloride solution with 1 times the theoretical molar content of sodium aluminate to the filtered sodium aluminate solution to obtain aluminum hydroxide precipitate, and continuously wash the aluminum hydroxide precipitate with 20°C ultrapure water until there is no white precipitate when a silver nitrate solution is dropped into the filtrate to obtain a precursor aluminum hydroxide, and calcine the dried precursor to obtain a high-purity aluminum oxide powder.

[0032] Comparative Example 2:

[0033] Add 30wt% sulfuric acid with 1 times the theoretical molar content of aluminum to 0.2mol of industrial aluminum hydroxide powder, stir in a magnetic stirrer for 40min to generate an aluminum sulfate solution, filter out impurities that cannot be dissolved and react to form silicic acid, add 30wt% sodium hydroxide solution to the filtered aluminum sulfate solution, set the pH to 14, and form a sodium aluminate solution. Filter out impurities in the sodium aluminate solution, add aluminum chloride solution with 1 times the theoretical molar content of sodium aluminate to the filtered sodium aluminate solution to obtain aluminum hydroxide precipitate, and continuously wash the aluminum hydroxide precipitate with 20°C ultrapure water until there is no white precipitate when a silver nitrate solution is dropped into the filtrate to obtain a precursor aluminum hydroxide, and calcine the dried precursor to obtain a high-purity aluminum oxide powder.

[0034] Comparative Example 3:

[0035] Add 30wt% sulfuric acid with 1.5 times the theoretical molar content of aluminum to 0.2mol of industrial aluminum hydroxide powder, set the temperature to 70°C in a magnetic stirrer, and heat for 40min to generate an aluminum sulfate solution. Filter out impurities that cannot be dissolved and react to form silicic acid, add 30wt% sodium hydroxide solution to the filtered aluminum sulfate solution, set the pH value to 11, and form a sodium aluminate solution. Filter out impurities in the sodium aluminate solution, add an aluminum chloride solution with 1 times the theoretical molar content of sodium aluminate to the filtered sodium aluminate solution, and obtain an aluminum hydroxide precipitate. The aluminum hydroxide precipitate is continuously washed with 70°C ultrapure water until there is no white precipitate when a silver nitrate solution is dripped into the filtrate to obtain a precursor aluminum hydroxide, and the dried precursor is calcined to obtain a high-purity aluminum oxide powder.

[0036] The high-purity aluminum oxide prepared in the embodiment and the comparative example was subjected to an ICP-OES performance test, and the contents of the impurity elements are shown in Table 1-2.

[0037] Table 1 Purity of aluminum oxide obtained in Examples 1-7

[0038] Example Na content (mg / kg) Fe content (mg / kg) Si content (mg / kg) purity% Example 1 453.28 6.51 470.00 99.907wt% Example 2 401.08 6.85 277.56 99.937wt% Example 3 243.96 6.08 609.64 99.915wt% Example 4 198.40 ND 110.30 99.969wt% Example 5 153.40 ND 336.60 99.948wt% Example 6 3.06 ND 17.93 99.998wt% Example 7 2.12 ND 18.72 99.998wt%

[0039] Note: ND means the content is too small to be detected.

[0040] Table 2 Purity of aluminum oxide obtained in Comparative Examples 1-3

[0041] Comparative Example Na content (mg / kg) Fe content (mg / kg) Si content (mg / kg) purity% Comparative Example 1 876.84 ND 445.97 99.867wt% Comparative Example 2 581.41 31.9 643.82 99.875wt% Comparative Example 3 582.62 ND 593.53 99.882wt%

[0042] Note: ND means the content is too small to be detected.

[0043] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A method for preparing high-purity aluminum oxide, include: (1) at room temperature, according to the mass of industrial aluminum hydroxide, 30 wt% dilute sulfuric acid is added, which is 1-2 times the theoretical molar content of aluminum, and heated and stirred in a magnetic stirrer to precipitate silicate ions in the aluminum hydroxide powder into silicic acid, and the precipitate in the solution is filtered to obtain an aluminum sulfate solution for use; (2) taking an aluminum sulfate solution, adding a sodium hydroxide solution at room temperature, adjusting the pH value, stirring the reaction, and allowing the iron ions to completely precipitate. After the reaction is complete, filtering the solution, and the aluminum sulfate solution reacts to generate a sodium aluminate solution; (3) Take a sodium aluminate solution, add an aluminum chloride solution with a theoretical molar content of 1-1.5 times that of aluminum, so that the aluminum ions are precipitated as white aluminum hydroxide precipitates, and the filtered precipitate is repeatedly washed with ultrapure water, and dried to obtain a high-purity aluminum oxide precursor aluminum hydroxide. After calcining the aluminum hydroxide, high-purity aluminum oxide is obtained.

2. The preparation method according to claim 1, in: The heating temperature of the magnetic stirrer in step (1) is 70-90° C., and the stirring time is 40-60 min.

3. The preparation method according to claim 1, in: The pH value of step (2) is adjusted to 12-14; The stirring reaction time is 5-10 min.

4. The preparation method according to claim 1, in: The ultrapure water used in step (3) has a temperature of 20-100°C.

5. The preparation method according to claim 1, in: The end point of the aluminum ion precipitation washing in step (3) is detected by silver nitrate solution. Chloride ions and silver ions react to form white precipitates. If white precipitates appear, it means that the chloride ions in the precursor have not been washed away. Washing should be continued until no white precipitates can be detected by silver nitrate.

6. A high-purity aluminum oxide obtained by the preparation method according to any one of claims 1 to 5.

Citation Information

Cited By

  • Method for preparing nanoscale aluminum oxide from industrial-grade aluminum hydroxide

    CN119706898A