Ultrathin flexible foldable cover plate glass and preparation method thereof

Ultra-thin flexible glass prepared through specific oxide ratios and process flow solves the problems of glass prone to cracking and poor durability in the prior art, and achieves the improvement of high flexibility and drop resistance, which is suitable for flexible electronic equipment.

CN119038872APending Publication Date: 2024-11-29SICHUAN HONGKE INNOVATION TECH CO LTD

Patent Information

Application Number
CN202411166852.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing ultra-thin flexible glass is prone to cracking during use, has poor durability, and edge cracks caused by cutting processes reduce the strength of the glass, affecting its foldable and chemical strengthening process.

Method used

Using glass preparation methods with specific oxide ratios, including high-temperature melting, polishing, precision annealing, etching and cutting and chemical reinforcement, to prepare ultra-thin flexible foldable cover glass with a thickness of less than 100μm, reduce edge cracks through polishing and improve glass flexibility and drop resistance.

Benefits of technology

It realizes the high flexibility and drop resistance of ultra-thin flexible glass, and is suitable for flexible electronic devices and foldable screen devices. It has passed all 200,000 bending tests, with excellent durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119038872A_ABST
    Figure CN119038872A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of ultrathin flexible glass, and particularly relates to ultrathin flexible foldable cover plate glass and a preparation method thereof. The glass comprises the following components in percentage by mass of oxides: 59 to 67 percent of SiO2, 16 to 23 percent of Al2O3, 7.5 to 16.5 percent of Na2O, 0 to 4.5 percent of MgO, 1 to 6.5 percent of B2O3 and 0 to 1 percent of SnO2. The thickness of the ultra-thin flexible foldable cover plate glass prepared by the method is less than or equal to 100 microns, the bending critical curvature radius is 1.2-1.5 mm, the pen falling impact height is 80-90 mm, and the ultra-thin flexible foldable cover plate glass passes 200,000 times of bending tests, has excellent flexibility and anti-falling performance, and can be well applied to the fields of flexible electronic equipment, foldable screen equipment, wearable display equipment and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of ultra-thin flexible glass, and specifically relates to an ultra-thin flexible foldable cover glass and a preparation method thereof. Background Art

[0002] In recent years, with the advent of foldable display devices, the development and production of ultra-thin and flexible glass, as well as the development and application of laminated materials composed of ultra-thin glass and polyimide (CPI) film, have been promoted. Although the foldable characteristics of the CPI cover are excellent, the protective function still has obvious disadvantages and the durability of the entire display module is poor. Due to the poor scratch resistance of CPI materials, scratches are prone to occur, and the impact protection ability is weak, and it cannot play a protective role when impacted by external forces. Therefore, the concept of flexible glass was proposed, which not only has the advantages of glass, but also its bendable characteristics make it possible to be used in foldable devices and flexible display devices. Electronic glass with a thickness of less than 100μm shows bendability and flexibility, and the smaller the thickness, the better the flexibility. Flexible ultra-thin glass is chemically strengthened to improve the glass strength, the number of bends and the wear resistance, making up for the shortcomings of flexible screens.

[0003] Flexible screens need to be bent and touched repeatedly during use. Ultra-thin flexible electronic glass cracks during the bending process and breaks due to accidental falling, which has become a common problem and affects the promotion and application of ultra-thin flexible electronic glass. In addition, the probability of the cover glass of the flexible screen contacting foreign objects is reduced when the flexible screen is folded, and the demand for the scratch resistance of the glass surface is reduced. The durability of flexible electronic glass can be effectively improved by improving the flexibility and drop resistance of the glass. How to improve the flexibility and drop resistance of ultra-thin flexible electronic glass is a technical problem that needs to be solved urgently. At present, foldable reality devices still have problems such as folding gaps, screen life, folding degree and creases, which need further research and improvement.

[0004] In the prior art, small-sized ultra-thin flexible glass is generally obtained by thinning large-sized glass and then cutting it. For example, when laser cutting is used, the thermal expansion and contraction caused by the temperature generated by laser cutting will also cause tiny cracks on the edges of the cut small-sized flat glass. Therefore, whether it is mechanical cutting or laser cutting, it is very easy for the glass to crack at the cut edge during cutting, and the cracks at the cut edge will greatly reduce the strength of the glass and make the glass unable to bend. Furthermore, during the chemical strengthening process of the glass with edge cracks, the cracks will rapidly expand under the action of stress, causing it to break and shatter. In view of this, there is an urgent need to improve the preparation process of small-sized ultra-thin flexible glass. Summary of the invention

[0005] One of the purposes of the present invention is to provide an ultra-thin flexible foldable cover glass in view of the problems existing in the prior art, wherein the glass can improve the flexibility and drop resistance of the ultra-thin flexible foldable cover glass.

[0006] In order to achieve the above invention objectives, the specific technical solution adopted by the present invention is:

[0007] An ultra-thin flexible foldable cover glass, whose components, expressed by oxide mass percentage, contain 59-67% SiO2, 16-23% Al2O3, 7.5-16.5% Na2O, 0-4.5% MgO, 1-6.5% B2O3, and 0-1% SnO2.

[0008] Further, preferably, an ultra-thin flexible foldable cover glass, whose components, expressed as percentage by mass of oxides, contain 61-65% SiO2, 18-21% Al2O3, 9.5-14.5% Na2O, 1-3% MgO, 2.5-5% B2O3, and 0.1-0.6% SnO2.

[0009] A second object of the present invention is to provide the above-mentioned method for ultra-thin flexible foldable cover glass, comprising the following steps:

[0010] Weigh each raw material according to the oxide ratio and mix them evenly to obtain a mixed raw material; load the mixed raw material into a (small) mixer, mix them in the mixer to obtain a complex mixture; pour the complex mixture into a platinum-rhodium crucible, and melt, clarify and homogenize it at high temperature (6-8h) in a (experimental small) high-temperature kiln at 1590-1680°C to obtain molten glass liquid; flatten and polish the molten glass liquid through a (experimental small) tin bath, and then enter an annealing furnace for precision annealing and cooling; finally, cut and grind the glass into a main glass plate with a thickness of 0.3mm and a size of 840×630mm, and polish the edge of the main glass plate; polishing the edge of the main glass can reduce cracks at the edge of the main glass and avoid the influence of cracks on subsequent thinning, cutting and strengthening processes. Since the present application is to prepare ultra-thin glass, the thickness of the glass after thinning is extremely small, so the cracks on the edge will directly affect the qualified rate of the final product.

[0011] An acid-resistant film is attached to the front side, i.e., the air side, of the main glass plate obtained after polishing to prevent it from being affected by the etching liquid during the etching and thinning process; the back side of the glass plate is then etched and thinned using the etching liquid to obtain an original ultra-thin flexible glass with a thickness of ≤100μm; after thinning, since the main glass itself has certain bending properties, the glass becomes the original ultra-thin flexible glass.

[0012] Continue to etch and cut the original ultra-thin flexible glass, then tear off the acid-resistant film to obtain the target glass;

[0013] The target glass is chemically strengthened, cooled and then cleaned to obtain an ultra-thin flexible foldable cover glass.

[0014] As a better implementation mode in the present application, in the method of ultra-thin flexible foldable cover glass, among the raw materials, SiO2 comes from ultra-pure sand; Al2O3 comes from aluminum oxide; Na2O comes from sodium carbonate and alum; MgO comes from magnesium oxide; B2O3 comes from boron oxide; SnO2 comes from tin oxide.

[0015] During precision annealing cooling, the annealing temperature is 600-650°C, the annealing time is 1-1.5h, and the homogenization time is 6-8h.

[0016] As a preferred embodiment of the present application, in the method for preparing ultra-thin flexible foldable cover glass, the polishing method includes any one of chemical polishing, flame polishing and mechanical polishing, and more preferably chemical polishing or flame polishing.

[0017] As a preferred embodiment of the present application, in the method for ultra-thin flexible foldable cover glass, the specific steps of etching and cutting are:

[0018] An acid-resistant film is attached to the front and back of the original ultra-thin flexible glass, and an acid-resistant film having a contour consistent with the target small-size (120×90mm) glass is attached. Subsequently, a contour line consistent with the shape of the target glass is engraved on the acid-resistant film, and the glass portion corresponding to the contour line is exposed outside the acid-resistant film. Then, an etching solution is used to etch through the glass portion corresponding to the contour line to obtain the target glass having the same shape as the contour line.

[0019] As a better implementation method in the present application, in the method of ultra-thin flexible foldable cover glass, the method of engraving a contour line on the acid-resistant film whose shape is consistent with the shape of the target glass is: ultraviolet etching or laser burning; the target minimum size is 120×90mm.

[0020] As a better embodiment of the present application, in the method of ultra-thin flexible foldable cover glass, the chemical strengthening conditions are: strengthening temperature 390-450°C, strengthening time 2-3.5h; molten salt is pure KNO3 molten salt. More preferably, the chemical strengthening conditions include: strengthening temperature 400-440°C, strengthening time 2.5-3h. Finally, the chemically strengthened glass sheet is immersed in warm water, washed and dried to obtain a strengthened ultra-thin flexible foldable cover glass.

[0021] The third object of the invention of the present application is to protect the ultra-thin flexible foldable cover glass that can be prepared by any of the above methods or combinations of method steps.

[0022] In the present invention, SiO2 is a key part of the ultra-thin flexible foldable cover glass, constituting the core material of the network skeleton structure of the glass. It is an important glass-forming oxide and exists in the form of [SiO4] tetrahedron. The SiO2 component gives the glass properties such as high mechanical strength, high chemical stability and low thermal expansion coefficient. SiO2 can simultaneously increase the elastic modulus and Vickers hardness value of electronic glass, so too low SiO2 concentration in the glass will lead to poor elastic modulus and chemical stability. In the embodiment, the SiO2 content is ≥59%; the SiO2 content is ≥61%. The melting point of SiO2 is 1713°C, which increases the viscosity of the glass, which is not conducive to glass clarification and ultra-thin forming. At the same time, the SiO2 component can quickly increase the Vickers hardness of the glass. Therefore, the SiO2 content in the glass is ≤67%, and the preferred content is ≤65%.

[0023] Al2O3 is an intermediate oxide. When the molar ratio of Na2O to Al2O3 in the glass is greater than 1, aluminum-oxygen tetrahedron [AlO4] is formed, and it forms a continuous structural network with silicon-oxygen tetrahedron. When the molar ratio of Na2O to Al2O3 is less than 1, octahedron [AlO6] is formed, which is an external body of the network and is located in the cavities of the silicon-oxygen structural network. Since the Al-O bond length is 0.176nm, the volume of the structural unit forming [AlO4] is 41cm 3 / mol, and the Si-O bond length is 0.16nm, and the volume of the [SiO4] structural unit formed is 27.2cm 3 / mol, the volume ratio of [AlO4] to [SiO4] is about 50%. When [AlO4] in the glass participates in the glass structure, the gaps in the glass network structure become larger, providing channels for ion exchange and accelerating ion exchange. Therefore, the Al2O3 content in the glass is ≥16%, and the Al2O3 content is preferably ≥18%. However, the melting point of Al2O3 oxide is 2050℃, which is an extremely refractory oxide, causing the viscosity of the glass to rise sharply, making it more difficult to clarify and homogenize the glass, resulting in a decrease in product yield, and increasing the difficulty of glass molding and thinning. Therefore, the Al2O3 content in the glass is ≤23%, preferably ≤21%.

[0024] B2O3 is a glass-forming oxide. It has boron-oxygen triangles [BO3] and boron-oxygen tetrahedrons [BO4] as structural units. It forms a structural network with silicon-oxygen tetrahedrons in borosilicate glass. B2O3 can reduce the expansion coefficient of glass, improve the thermal and chemical stability of glass, improve the gloss of glass, and improve the mechanical properties of glass. B2O3 also acts as a flux to accelerate the melting and clarification of glass. However, B2O3 is a volatile component, which can easily lead to uneven glass composition and reduce the strength of glass. Too high B2O3 leads to poor chemical stability of glass. The B2O3 content is ≤6.5%, preferably ≤5%.

[0025] Na2O is a network oxide that destroys the network structure of glass, effectively improves glass melting and clarification, and also reduces the Vickers hardness of glass. In KNO3 molten salt above 350℃, Na2O in glass + K in the enhanced molten salt + Ion exchange occurs, forming surface compressive stress on the glass surface, effectively improving the mechanical strength of the ultra-thin flexible foldable cover glass. The Na2O content is ≥7%, and the Na2O content is ≥9.5%. Excessive Na2O will cause a series of performance deteriorations of the glass, such as a significant reduction in the mechanical properties of the glass and a reduction in the chemical resistance of the glass. The Na2O content is ≤16.5%, preferably ≤14.5%.

[0026] MgO is a divalent cation oxide, a network exosome, which promotes the melting and melting of glass, and improves the mechanical properties of glass. At the same time, the addition of MgO is beneficial to the internal filling of the network structure, consolidates the network body, improves the scratch resistance of glass, and MgO can increase the elastic modulus and Vickers hardness of glass, reduce the crystallization tendency of glass, improve the forming performance of glass, and facilitate the forming operation. The MgO content in the ultra-thin flexible foldable cover glass of the present invention is ≤4.5%, and preferably the MgO content is ≤3%.

[0027] The ultra-thin flexible glass of the present invention contains a clarifier, which includes SnO2 and Na2SO4, wherein SnO2 is 0-1%, preferably 0.1-0.6%, and is mainly used for high-temperature clarification during glass melting, improving glass clarification effect and reducing internal defect rate of glass.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] (1) The glass of the present invention has excellent performance and can be well applied to the fields of flexible electronic devices, foldable screen devices and wearable display devices;

[0030] (ii) The thickness of the ultra-thin flexible foldable cover glass prepared by this method is ≤100 μm, and its thermal expansion coefficient is 83.1-86.1×10 -7 / ℃, density is 2.39-2.44g / cm 3 , Vickers hardness is 607-661Kgf / mm 2 , elastic modulus is 86.97-87.21Gpa; surface compressive stress value-CS is 663-699Mpa, compressive stress layer depth-DOL is 13.5-15.8μm, critical curvature radius of bending is 1.2-1.5mm, pen impact height is 80-90mm, 200,000 bending tests have all been passed, with excellent flexibility and drop resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 The present invention is a schematic diagram of an ultra-thin flexible foldable cover glass and a method for preparing the same. DETAILED DESCRIPTION

[0032] The following is a detailed description of the implementation of the ultra-thin flexible foldable cover glass of the present invention, but the present invention is not limited to the following implementation, and can be implemented with appropriate changes within the scope of the purpose of the present invention. In addition, although there are appropriate omissions in the repeated description, the main purpose of the invention will not be limited by this. In the following content, the ultra-thin flexible foldable cover glass of the present invention is sometimes referred to as glass.

[0033] Explain the physical properties and performance test methods of glass samples:

[0034] (1) Softening point temperature (107.6P), measured according to GB / T28195-2011 "Test method for softening point of glass"; (2) Annealing point temperature (1013P), measured by expansion curve using a dilatometer; (3) Strain point temperature (1014.5P), measured by expansion curve using a dilatometer; (4) Thermal expansion coefficient, measured according to GB / T16920-2015 "Determination of average linear thermal expansion coefficient of glass"; (5) (6) Elastic modulus, measured by using a micro Vickers hardness tester in accordance with the standard GB / T16534-2009, with a loading force of 200 g and a loading time of 10 s; (7) Thermal expansion coefficient, measured by using GB / T16920-2015 Determination of average linear thermal expansion coefficient of glass; (8) Surface The surface compressive stress value (CS) and the depth of the compressive stress layer (DOL) were measured by using a surface stress meter (FSM-6000LE) in accordance with the method described in standard GB / T18144-2008; (9) Static limit bending curvature radius: The limit bending radius R was tested in accordance with GB / T38686-2020 "Ultra-μm, Thin Glass Flexibility Test Method Two-point Bending Method"; (10) Displacement bending test: The test was conducted using a U-shaped bending test machine. The test method was a downward pressure height of 3 mm, a radius R of 1.5 mm, a left and right movement of 10-15 mm, a movement speed of 5-10 mm / min, and PET film (20 μm PSA + 50 μm PET) was pasted on both sides; (11) Pen impact height: The test was conducted using a pen test machine. The test method was to allow a 12 g signature pen (bead core diameter 0.5 mm) to fall freely on the glass (UTG + 20 μm PSA + 50 μm PET) to check the pen penetration ability.

[0035] Specific conditions not specified in this application were carried out according to conventional conditions or conditions recommended by the manufacturer. Reagents or instruments used without indicating the manufacturer were conventional products that can be purchased commercially.

[0036] The following is an explanation of the range of each component (ingredient) of the ultra-thin flexible foldable cover glass of the present invention. In this specification, unless otherwise specified, the content of each component is expressed in weight percentage (wt%) relative to the total amount of glass material converted into an oxide composition. Here, the "composition converted into oxides" means that when oxides, complex salts, hydroxides, etc. used as raw materials for the ultra-thin flexible foldable cover glass components of the present invention decompose and transform into oxides when melted, the total amount of the oxide material is taken as 100%.

[0037] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0038] Example

[0039] The present invention is described below with reference to specific embodiments. It should be noted that these embodiments are merely illustrative and do not limit the present invention in any way.

[0040] In order to obtain an ultra-thin flexible foldable cover glass having a composition shown in Tables 1 and 2, the oxides in the table are used as raw materials, and each raw material (each raw material is: ultra-pure sand, aluminum oxide, sodium carbonate, magnesium oxide, boron oxide, tin oxide, and sodium sulfate) is weighed according to the oxide ratio and mixed evenly to obtain a mixed raw material; the mixed raw material is loaded into a (small) mixer, and mixed in the mixer to obtain a complex mixture; the complex mixture is poured into a platinum-rhodium crucible, and high-temperature melting, clarification and homogenization are carried out in an experimental small high-temperature kiln to obtain a molten glass liquid, and the melting system is: heating to 1550°C within 2.5 hours, keeping warm at 1500°C for 1 hour, then heating to 1680°C within 0.5 hours, and keeping warm at 1680°C for 3.5 hours before discharging; the molten glass liquid is The molten glass liquid is flattened and polished through a (small experimental) tin bath, and then enters an annealing furnace for precision annealing and cooling; finally, the glass is cut and ground into a main body glass plate with a thickness of 0.3mm and a size of 840×630mm, and the edge of the main body glass plate is polished (the polishing method includes chemical polishing); the front side of the main body glass plate obtained after polishing, that is, the air side, is attached with an acid-resistant film to prevent it from being affected by the etching liquid during the etching and thinning process; then the back side of the glass plate is etched and thinned with an etching liquid to obtain an original ultra-thin flexible glass with a thickness of ≤100μm; after thinning, since the main body glass itself has certain bending properties, the glass becomes the original ultra-thin flexible glass. Continue to etch and cut the original ultra-thin flexible glass, then tear off the acid-resistant film to obtain the target glass; chemically strengthen the target glass, cool it, and then clean it to obtain an ultra-thin flexible foldable cover glass.

[0041] The specific steps of etching and cutting are:

[0042] An acid-resistant film is attached to the front and back of the original ultra-thin flexible glass, and an acid-resistant film having a contour consistent with the target small-size (120×90mm) glass is attached. Subsequently, a contour line consistent with the shape of the target glass is engraved on the acid-resistant film by ultraviolet etching, and the glass portion corresponding to the contour line is exposed outside the acid-resistant film. Then, an etching solution is used to etch through the glass portion corresponding to the contour line to obtain the target glass having the same shape as the contour line.

[0043] The chemical strengthening conditions include: a strengthening temperature of 420° C. and a strengthening time of 3 hours and 40 minutes. Finally, the chemically strengthened glass sheet is immersed in warm water, and after cleaning and drying, a strengthened ultra-thin flexible foldable cover glass is obtained.

[0044] In addition, the properties of each glass were measured by the method shown above, and the measurement results are shown in Tables 1 and 2.

[0045] Table 1: Comparison of the composition and physical properties of ultra-thin flexible foldable cover glass Examples 1-8 and Comparative Examples 1-4

[0046]

[0047]

[0048] It can be seen from Table 1 that the thermal expansion coefficient of the ultra-thin flexible foldable cover glass prepared in the embodiment of the present invention is 83.1-86.1×10 -7 / ℃, density is 2.39-2.44g / cm 3 , Vickers hardness is 607-661Kgf / mm 2 , the elastic modulus is 86.97-87.21 GPa; the thermal expansion coefficient of the ultra-thin flexible foldable cover glass prepared by the present invention is 90.07-91.74×10 -7 / ℃, density is 2.45-2.46g / cm 3 , Vickers hardness is 517-543Kgf / mm 2 , the elastic modulus is 70.51-70.97 GPa; and the four physical property parameters of the embodiments of the present invention listed above are all better than those of the comparative examples of the present invention.

[0049] Table 2 Performance test comparison of ultra-thin flexible foldable cover glass Examples 1-8 and Comparative Examples 1-4

[0050]

[0051] It can be seen from Table 2 that the surface compressive stress value -CS of the ultra-thin flexible foldable cover glass prepared in the embodiment of the present invention is 663-699Mpa, the depth of the compressive stress layer -DOL is 14.6-16.8μm, the critical curvature radius of bending is 1.2-1.5mm, the pen impact height is 80-90mm, 300,000 static limit bending tests are all passed, the offset bending test is all passed, and the drop ball test height is 100-110cm; the surface compressive stress value -CS of the ultra-thin flexible foldable cover glass prepared in the comparative example of the present invention is 511-527Mpa, the depth of the compressive stress layer -DOL is 12.4-13.3μm, the critical curvature radius of bending is 6-7mm, the pen impact height is 50-60mm, 300,000 static limit bending tests are all failed, the offset bending test is all failed, and the drop ball test height is 70-80cm; and the seven performance test items of the embodiments of the present invention listed above are all significantly better than the comparative example of the present invention.

[0052] The above-mentioned embodiments only express the specific implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the protection scope of the present application. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the technical solution concept of the present application, and these all belong to the protection scope of the present application.

[0053] This background section is provided to generally present the context of the invention, and the work of the presently named inventors, the work to the extent described in this background section, and aspects of this section that did not constitute prior art at the time of application are neither explicitly nor implicitly admitted to be prior art to the present invention.

Claims

1. An ultra-thin flexible foldable cover glass, characterized in that: Its components, expressed in terms of oxide mass percentage, contain 59-67% SiO2, 16-23% Al2O3, 7.5-16.5% Na2O, 0-4.5% MgO, 1-6.5% B2O3, and 0-1% SnO2.

2. The ultra-thin flexible foldable cover glass according to claim 1, characterized in that: Its components, expressed in terms of oxide mass percentage, contain 61-65% SiO2, 18-21% Al2O3, 9.5-14.5% Na2O, 1-3% MgO, 2.5-5% B2O3, and 0.1-0.6% SnO2.

3. The method for preparing the ultra-thin flexible foldable cover glass according to claim 1 or 2, characterized in that The following steps are involved: Weigh each raw material according to the oxide ratio and mix them evenly to obtain a mixed raw material; put the mixed raw material into a mixer, mix them evenly in the mixer to obtain a complex mixture; pour the complex mixture into a platinum-rhodium crucible, melt, clarify and homogenize it in a high-temperature kiln at 1590-1680°C to obtain molten glass liquid; flatten and polish the molten glass liquid through a tin bath, and then enter an annealing furnace for precision annealing and cooling; finally, cut and grind the glass into a main body glass plate with a thickness of 0.3 mm and a size of 840×630 mm, and polish the edge of the main body glass plate; An acid-resistant film is attached to the front of the main glass plate obtained after the polishing treatment, and then the back of the glass plate is etched and thinned by using an etching liquid to obtain an original ultra-thin flexible glass with a thickness of ≤100 μm; the original ultra-thin flexible glass is further etched and cut, and then the acid-resistant film is torn off to obtain the target glass; The target glass is chemically strengthened, cooled and then cleaned to obtain an ultra-thin flexible foldable cover glass.

4. The method for preparing the ultra-thin flexible foldable cover glass according to claim 3, characterized in that: Among the raw materials, SiO2 comes from ultra-pure sand; Al2O3 comes from alumina; Na2O comes from sodium carbonate and sodium sulfate; MgO comes from magnesium oxide; B2O3 comes from boron oxide; and SnO2 comes from tin oxide.

5. The method for preparing the ultra-thin flexible foldable cover glass according to claim 3 or 4, characterized in that: During precision annealing cooling, the annealing temperature is 600-650°C, the annealing time is 1-1.5h, and the homogenization time is 6-8h.

6. The method for preparing the ultra-thin flexible foldable cover glass according to claim 5, characterized in that: The polishing method includes any one of chemical polishing, flame polishing and mechanical polishing.

7. The method for preparing the ultra-thin flexible foldable cover glass according to claim 3, 4 or 5, characterized in that: The specific steps of etching and cutting are: An acid-resistant film is attached to the front and back sides of the original ultra-thin flexible glass, and an acid-resistant film having a contour consistent with the target small-sized glass is attached. Subsequently, a contour line consistent with the shape of the target glass is engraved on the acid-resistant film, and the glass portion corresponding to the contour line is exposed outside the acid-resistant film. Then, an etching solution is used to etch through the glass portion corresponding to the contour line to obtain the target glass having the same shape as the contour line.

8. The method for preparing the ultra-thin flexible foldable cover glass according to claim 7, characterized in that: The method for carving a contour line with a shape consistent with the target glass shape on the acid-resistant film is: ultraviolet etching or laser burning; the minimum size of the target is 120×90 mm.

9. The method for preparing the ultra-thin flexible foldable cover glass according to claim 3, 4, 6 or 8, characterized in that: The conditions for chemical strengthening are: strengthening temperature 390-450°C, strengthening time 2-3.5h; the molten salt is pure KNO3 molten salt.

10. An ultra-thin flexible foldable cover glass prepared according to the method of claim 9.

Citation Information

Patent Citations

  • Composition for glass, glass as well as preparation method and application of glass

    CN107827352A

  • Thin glass with improved bendability and chemical toughenability

    CN111094199A

  • Anti-bending glass as well as preparation method and application thereof

    CN116947316A

  • Ultrathin flexible tempered glass and preparation method thereof

    CN117776519A

Cited By

  • Ultrathin glass, reinforced impact-resistant ultrathin glass and preparation method and application thereof

    CN120271224A

  • Ultra-thin glass and strengthened impact-resistant ultra-thin glass, preparation method therefor, and use thereof

    WO2026179251A1