Low-heat Portland cement clinker with early strength characteristic and preparation method thereof

By changing the mineral structure and incorporating mineral agents into low-thermal silicate cement clinker, the balance of early strength, late strength stability and low heat release are solved, and the early strength and late stability of concrete are significantly improved. Reduce temperature crack problems and improve project quality and safety.

CN119038892AInactive Publication Date: 2024-11-29JIAHUA SPECIAL CEMENT
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410973221.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing low-thermal silicate cement has shortcomings in quickly reaching design strength and controlling the internal temperature rise of concrete, making it difficult to balance early strength, late-stage strength stability and low heat release.

Method used

By adding mineralizers to low-thermal silicate cement clinker, the size and structure of ore A (C3S) and ore B (C2S) are changed, the liquid phase viscosity is reduced, the calcination reaction activity is improved, and the early strength of the cement is significantly improved. Maintain stable growth of intensity in the later stage, while controlling heat release during hydration.

Benefits of technology

It significantly improves the early strength of concrete, shortens the construction cycle, ensures stable growth of strength in the later stage, reduces temperature crack problems, and improves project quality and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119038892A_ABST
    Figure CN119038892A_ABST
Patent Text Reader

Abstract

The invention discloses a low-heat Portland cement clinker with an early strength characteristic and a preparation method thereof. The cement clinker comprises the following raw materials in percentage by mass: 60-85% of a calcium raw material; 2 to 20 wt.% of a siliceous raw material; 1-10 wt.% of an aluminum raw material; 1-10 wt.% of an iron correction raw material; 0.1 to 5 wt.% of a mineralizing agent; the mineralizer is at least one of fluorgypsum, phosphogypsum, fluorine slag, manganese slag, yellow phosphorus slag, copper slag and zinc slag. According to the invention, a special process is adopted to control the mineral phase transformation in the clinker sintering process, so that the sizes and structures of C3S and C2S in the low-heat Portland cement are changed, the early strength of the cement is improved, the characteristic of low hydration heat is maintained, the internal temperature rise of the concrete is reduced, temperature cracks are prevented, and the overall quality and safety of a project are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, and in particular to a low-heat silicate cement clinker with early strength characteristics and a preparation method thereof. Background Art

[0002] In the rapidly developing modern construction industry, as one of the most basic building materials, the optimization and improvement of cement performance has always been a key factor in promoting the progress of engineering technology. With the continuous emergence of complex engineering structures such as high-rise buildings, large bridges, tunnels, and nuclear power plants, the performance requirements for building materials, especially cement materials, are increasing day by day.

[0003] Low-heat silicate cement is composed of dicalcium silicate (C2S) as the main mineral. Although it has good performance in terms of low heat, high late strength, low shrinkage, and high corrosion resistance, its performance is slightly insufficient in certain specific application scenarios, such as the need to quickly reach the design strength to shorten the construction period, or the need to strictly control the temperature rise inside the concrete to prevent temperature cracks.

[0004] In view of the limitations of silicate cement, domestic and foreign scholars and research institutions have launched relevant research, aiming to develop new types of cement with better performance by improving the raw material ratio, optimizing the calcination process, adding admixtures, etc. Among them, the research directions of early strength cement, low heat cement and cement for high performance concrete are particularly eye-catching. However, the early strength cement currently available on the market often has problems such as insufficient later strength development and easy cracking; while low heat cement may sacrifice strength performance in some aspects. Therefore, how to balance the early strength, later strength stability and low heat release of cement has become a technical problem that needs to be solved urgently. Summary of the invention

[0005] The present invention provides a low-heat silicate cement clinker with early strength characteristics and a preparation method thereof. Compared with the low-heat cement clinker on the market, the low-heat silicate cement clinker prepared by the method changes the size and structure of A ore (C3S) and B ore (C2S) in the low-heat silicate cement, increases the hydration reaction activity of A ore and B ore, and increases the compressive strength of the cement at 3d and 28d by 25% and 12% respectively (improved early construction performance).

[0006] The technical problem to be solved by the present invention is to balance the early strength, late strength stability and low heat release of low heat cement. By changing the mineral structure of low heat cement clinker, the early strength is significantly improved to meet the needs of rapid construction, while maintaining a stable growth in the late strength development, and the heat released during the entire hydration process is relatively low, which helps to reduce the problem of temperature cracks in large-volume concrete construction and improve the overall quality and safety of the project.

[0007] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0008] A low-heat silicate cement clinker with early strength characteristics, comprising the following raw materials in percentage by mass:

[0009] Calcium raw material: 60-85wt.%;

[0010] Siliceous raw material: 2-20wt.%;

[0011] Aluminum raw material: 1-10wt.%;

[0012] Iron correction raw material: 1-10wt.%;

[0013] Mineralizer: 0.1-5wt.%;

[0014] The mineralizer is at least one of fluorite, phosphogypsum, fluorine slag, manganese slag, yellow phosphorus slag, copper slag and zinc slag.

[0015] The present invention effectively reduces the liquid phase viscosity during the clinker formation process and significantly improves the activity of the calcination reaction by adding a mineralizer. This improvement not only promotes the formation of the mineral phase, but also changes the size and structure of the A ore (C3S) and the B ore (C2S) in the mineral phase, accelerates the initial process of cement hydration reaction, significantly improves the early strength of concrete, and shortens the construction period.

[0016] In some embodiments of the present invention, the cement clinker comprises the following raw materials in percentage by mass:

[0017] Calcium raw material: 70-80wt.%;

[0018] Siliceous raw material: 5-15wt.%;

[0019] Aluminum raw material: 2-7wt.%;

[0020] Iron correction raw material: 2-7wt.%;

[0021] Mineralizer: 0.5-2wt.%;

[0022] The mineralizer is at least one of fluorite, phosphogypsum, fluorine slag, manganese slag, yellow phosphorus slag, copper slag and zinc slag.

[0023] Furthermore, the size of tricalcium silicate in the cement clinker is 40-100 μm, and the size of dicalcium silicate is 5-30 μm.

[0024] Furthermore, the calcium raw material is any one or more of limestone, calcite, chalk and carbide slag.

[0025] Furthermore, the siliceous raw material is any one or more of quartz, silica, red sand and sandstone.

[0026] Furthermore, the aluminum raw material is any one or more of clay, red mud, and shale.

[0027] Furthermore, the iron correction raw material is any one or more of non-ferrous metal ash, iron powder, steel slag, and iron ore waste slag.

[0028] Furthermore, the clinker rate values ​​of the cement clinker are: lime saturation coefficient 0.75-0.84, silicon rate 2.20-2.70, and aluminum rate 0.64-1.20.

[0029] The present invention also provides a method for preparing low-heat silicate cement clinker with early strength characteristics, comprising the following steps:

[0030] Step 1, mix the raw materials evenly according to the proportion, grind and sieve to obtain cement raw material powder;

[0031] Step 2, adding 10% water by mass of the cement raw material powder to the cement raw material powder, pressing it into a test cake of Φ11.5cm×1cm at a pressure of 25±5MPa, wherein one side of the test cake has corrugations and weighs 105±5g, and drying the test cake to a constant weight, wherein the corrugations are to ensure heat transfer during firing;

[0032] Step 3, calcining the dried test cake, the calcination includes the following stages: calcining at room temperature to 950°C for 30 minutes, keeping at 950°C for 30 minutes, calcining at 950°C to 1450°C for 30 minutes, keeping at 1450°C for 30 minutes, then taking out and cooling to obtain the cement clinker.

[0033] Furthermore, in the step 1, the residue is ≤18% by using a 80 um square hole sieve.

[0034] Compared with the prior art, the present invention has the following beneficial effects:

[0035] 1. Early strength characteristics: By changing the size and structure of A ore (C3S) and B ore (C2S) in low-heat silicate cement, the initial process of cement hydration reaction is accelerated, the early strength of concrete is significantly improved, and the construction period is shortened. The specific changes are as follows:

[0036] (1) The size of tricalcium silicate (C3S) in traditional low-heat silicate cement clinker is about 10-60 μm. The size of tricalcium silicate in the cement clinker prepared by the present invention becomes larger, about 40-100 μm, and has a cavitation structure, which is more susceptible to mechanical damage during grinding, thereby breaking the original structure and increasing the activity of the hydration reaction.

[0037] (2) The size of dicalcium silicate (C2S) in traditional low-heat silicate cement clinker is about 20-40 μm. The size of dicalcium silicate in the cement clinker prepared by the present invention becomes smaller, about 5-30 μm, and the outline of dicalcium silicate becomes smoother. Under the condition of the same dicalcium silicate mass ratio, the amount of dicalcium silicate is greater, and its amount also increases exponentially, thereby increasing the hydration contact interface of dicalcium silicate and improving the hydration rate.

[0038] 2. Stable strength in the later stage: It is ensured that during long-term use, the cement clinker of the present invention can continue to provide stable strength growth to meet the long-term bearing requirements of the project. It is particularly suitable for engineering fields with high requirements for early strength, stable strength growth in the later stage and the need to control temperature rise, such as high-rise buildings, bridges, tunnels, nuclear power plants and other large-volume concrete structure construction.

[0039] 3. Low heat release: The present invention adopts a special process to control the mineral phase transformation during the clinker burning process, which improves the early strength of cement while maintaining the characteristics of low hydration heat, reduces the internal temperature rise of concrete, prevents temperature cracks, and improves the overall quality and safety of the project. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 This is a distribution diagram of the mineral structure morphology of the low-heat Portland cement clinker of the present invention.

[0041] Figure 2 This is the mineral structure morphology distribution diagram of low-heat Portland cement clinker on the market. DETAILED DESCRIPTION

[0042] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0043] In the embodiment of the present invention, the mineralizer is at least one of fluorite, phosphogypsum, fluorine slag, manganese slag, yellow phosphorus slag, copper slag and zinc slag.

[0044] In the embodiment of the present invention, the calcium raw material is any one or more of limestone, calcite, chalk and carbide slag.

[0045] In the embodiment of the present invention, the siliceous raw material is any one or more of quartz, silica, red sand and sandstone.

[0046] In the embodiment of the present invention, the aluminum raw material is any one or more of clay, red mud, and shale.

[0047] In the embodiment of the present invention, the iron correction raw material is any one or more of non-ferrous metal ash, iron powder, steel slag, and iron ore waste slag.

[0048] The method for preparing cement clinker in the embodiment of the present invention comprises the following steps:

[0049] Step 1, mix all raw materials in proportion, grind and sieve to obtain cement raw material powder, and sieve with a 80um square hole sieve to obtain a sieve residue of ≤18%;

[0050] Step 2, adding 10% water by mass of the cement raw material powder to the cement raw material powder, pressing the mixture into a test cake of Φ11.5 cm×1 cm at a pressure of 25±5 MPa, wherein one side of the test cake has corrugations and weighs 105±5 g, and drying the test cake (at 105° C. for at least 2 hours) to constant weight;

[0051] Step 3, calcining the dried test cake, the calcination includes the following stages: calcining at room temperature to 950°C for 30 min, keeping at 950°C for 30 min, calcining at 950°C to 1450°C for 30 min, keeping at 1450°C for 30 min, then taking out and cooling to obtain cement clinker.

[0052] Example 1

[0053] As a preferred embodiment of the present invention, the composition of a low-heat silicate cement clinker with early strength characteristics disclosed in this embodiment is shown in Table 1.

[0054] Table 1

[0055] raw material Mass percentage (wt%) Calcium raw materials 77.3 Silica raw materials 13.9 Aluminum raw materials 3.1 Iron correction material 5.2 Mineralizer 0.5

[0056] The clinker rate values ​​of the cement clinker in this embodiment are: lime saturation coefficient 0.79±0.02, silicon rate 2.6±0.1, and aluminum rate 0.8±0.1.

[0057] The size of tricalcium silicate minerals in the cement clinker of this embodiment is 50-90 μm, and the size of dicalcium silicate minerals is 8-30 μm.

[0058] The cement clinker of the embodiment of the present invention is mixed with gypsum of 5% by mass of the cement clinker and mixed evenly to a specific surface area of ​​350±10m 2 / kg, low heat silicate cement is obtained.

[0059] Example 2

[0060] As a preferred embodiment of the present invention, the composition of a low-heat silicate cement clinker with early strength characteristics disclosed in this embodiment is shown in Table 2.

[0061] Table 2

[0062] raw material Mass percentage (wt%) Calcium raw materials 77.1 Silica raw materials 13.7 Aluminum raw materials 3.1 Iron correction material 5.1 Mineralizer 1.0

[0063] The clinker rate values ​​of the cement clinker in this embodiment are: lime saturation coefficient 0.79±0.02, silicon rate 2.6±0.1, aluminum rate 0.8±0.1

[0064] The size of tricalcium silicate minerals in the cement clinker of this embodiment is 60-90 μm, and the size of dicalcium silicate minerals is 2-25 μm.

[0065] The cement clinker of the embodiment of the present invention is mixed with gypsum of 5% by mass of the cement clinker and mixed evenly to a specific surface area of ​​350±10m 2 / kg, low heat silicate cement is obtained.

[0066] Example 3

[0067] As a preferred embodiment of the present invention, the composition of a low-heat silicate cement clinker with early strength characteristics disclosed in this embodiment is shown in Table 3.

[0068] Table 3

[0069] raw material Mass percentage (wt%) Calcium raw materials 76.0 Silica raw materials 13.8 Aluminum raw materials 3.0 Iron correction material 5.2 Mineralizer 2.0

[0070] The clinker rate values ​​of the cement clinker in this embodiment are: lime saturation coefficient 0.79±0.02, silicon rate 2.6±0.1, aluminum rate 0.8±0.1

[0071] The size of tricalcium silicate minerals in the cement clinker of this embodiment is 50-90 μm, and the size of dicalcium silicate minerals is 10-30 μm.

[0072] The cement clinker of the embodiment of the present invention is mixed with gypsum of 5% by mass of the cement clinker and mixed evenly to a specific surface area of ​​350±10m 2 / kg, low heat silicate cement is obtained.

[0073] Example 4

[0074] As a preferred embodiment of the present invention, the composition of a low-heat silicate cement clinker with early strength characteristics disclosed in this embodiment is shown in Table 4.

[0075] Table 4

[0076] raw material Mass percentage (wt%) Calcium raw materials 75.7 Silica raw materials 13.6 Aluminum raw materials 2.9 Iron correction material 4.8 Mineralizer 3.0

[0077] The clinker rate values ​​of the cement clinker in this embodiment are: lime saturation coefficient 0.79±0.02, silicon rate 2.6±0.1, aluminum rate 0.8±0.1

[0078] The size of tricalcium silicate minerals in the cement clinker of this embodiment is 60-100 μm, and the size of dicalcium silicate minerals is 5-20 μm.

[0079] The cement clinker of the embodiment of the present invention is mixed with gypsum of 5% by mass of the cement clinker and mixed evenly to a specific surface area of ​​350±10m 2 / kg, low heat silicate cement is obtained.

[0080] Example 5

[0081] As a preferred embodiment of the present invention, the composition of a low-heat silicate cement clinker with early strength characteristics disclosed in this embodiment is shown in Table 5.

[0082] Table 5

[0083]

[0084]

[0085] The clinker rate values ​​of the cement clinker in this embodiment are: lime saturation coefficient 0.79±0.02, silicon rate 2.6±0.1, aluminum rate 0.8±0.1

[0086] The size of tricalcium silicate minerals in the cement clinker of this embodiment is 50-95 μm, and the size of dicalcium silicate minerals is 10-25 μm.

[0087] The cement clinker of the embodiment of the present invention is mixed with gypsum of 5% by mass of the cement clinker and mixed evenly to a specific surface area of ​​350±10m 2 / kg, low heat silicate cement is obtained.

[0088] The physical properties of the low heat silicate cement in each embodiment were tested, and the same specific surface area (350m 2 / kg) of low-heat silicate cement was used as a comparative example, and the results are shown in Table 6.

[0089] Table 6

[0090]

[0091] According to Table 6, the silicate cement prepared from the cement clinker of the present invention is compared with the low-heat silicate cement on the market: the standard consistency is similar, the stability is qualified, but the setting time is shortened, the 3d hydration heat is slightly reduced, and the 3d strength and 28d strength are significantly enhanced, indicating that the silicate cement of the present invention can help reduce the temperature crack problem in the construction of large-volume concrete and improve the overall quality and safety of the project.

[0092] Depend on Figure 1 and Figure 2It can be seen that compared with the low-heat Portland cement clinker on the market, the size of tricalcium silicate (C3S) in the cement clinker of the present invention is larger than the size of tricalcium silicate (C3S) in the low-heat Portland cement clinker on the market, while the size of dicalcium silicate (C2S) is smaller than the size of dicalcium silicate (C2S) in the low-heat Portland cement clinker on the market.

[0093] Finally, it should be noted that the above embodiments are only preferred embodiments of the present invention to illustrate the technical solutions of the present invention, rather than limiting them, and certainly not limiting the patent scope of the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions recorded in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. These modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. In other words, any changes or modifications made to the main design concept and spirit of the present invention that have no substantive significance, and the technical problems they solve are still consistent with the present invention, should be included in the protection scope of the present invention. In addition, the direct or indirect application of the technical solutions of the present invention in other related technical fields is also included in the patent protection scope of the present invention.

Claims

1. A low-heat Portland cement clinker with early strength characteristics, characterized in that: The following raw materials are included in percentage by mass: Calcium raw material: 60-85wt.%; Siliceous raw material: 2-20wt.%; Aluminum raw material: 1-10wt.%; Iron correction raw material: 1-10wt.%; Mineralizer: 0.1-5wt.%; The mineralizer is at least one of fluorite, phosphogypsum, fluorine slag, manganese slag, yellow phosphorus slag, copper slag and zinc slag.

2. The low-heat silicate cement clinker with early strength characteristics according to claim 1, characterized in that: The following raw materials are included in percentage by mass: Calcium raw material: 70-80wt.%; Siliceous raw material: 5-15wt.%; Aluminum raw material: 2-7wt.%; Iron correction raw material: 2-7wt.%; Mineralizer: 0.5-2wt.%; The mineralizer is at least one of fluorite, phosphogypsum, fluorine slag, manganese slag, yellow phosphorus slag, copper slag and zinc slag.

3. A low-heat Portland cement clinker with early strength characteristics according to claim 1 or 2, characterized in that: The size of tricalcium silicate in the cement clinker is 40-100 μm, and the size of dicalcium silicate is 5-30 μm.

4. A low-heat Portland cement clinker with early strength characteristics according to claim 1 or 2, characterized in that: The calcium raw material is any one or more of limestone, calcite, chalk and carbide slag.

5. A low-heat Portland cement clinker with early strength characteristics according to claim 1 or 2, characterized in that: The siliceous raw material is any one or more of quartz, silica, red sand and sandstone.

6. A low-heat Portland cement clinker with early strength characteristics according to claim 1 or 2, characterized in that: The aluminum raw material is any one or more of clay, red mud and shale.

7. A low-heat Portland cement clinker with early strength properties according to claim 1 or 2, characterized in that: The iron correction raw material is any one or more of non-ferrous metal ash, iron powder, steel slag, and iron ore waste slag.

8. The low-heat Portland cement clinker with early strength characteristics according to claim 1 or 2, characterized in that: The clinker rate values ​​of the cement clinker are: lime saturation coefficient 0.75-0.84, silicon rate 2.20-2.70, and aluminum rate 0.64-1.

20.

9. A method for preparing low-heat Portland cement clinker with early strength characteristics according to any one of claims 1 to 8, characterized in that: The following steps are involved: Step 1, mix the raw materials evenly according to the proportion, grind and sieve to obtain cement raw material powder; Step 2, adding 10% water by mass of the cement raw material powder to the cement raw material powder, pressing the mixture into a test cake of Φ11.5 cm×1 cm at a pressure of 25±5 MPa, wherein one side of the test cake has corrugations and weighs 105±5 g, and drying the test cake to a constant weight; Step 3, calcining the dried test cake, the calcination includes the following stages: calcining at room temperature to 950°C for 30 minutes, keeping at 950°C for 30 minutes, calcining at 950°C to 1450°C for 30 minutes, keeping at 1450°C for 30 minutes, then taking out and cooling to obtain the cement clinker.

10. The method for preparing low-heat Portland cement clinker with early strength characteristics according to claim 9, characterized in that: In the step 1, the residue is ≤18% by sieving with a 80 μm square hole sieve.

Citation Information

Patent Citations

  • Mineral crystal of cement clinker and preparation method thereof

    CN104944812A