Composite water reducing agent for UHPC (Ultra High Performance Concrete) ultra-strong photovoltaic pipe pile material and preparation method of composite water reducing agent
By combining modified polycarboxylic acid water reducing agent and lignin and other compounds, a composite water reducing agent for UHPC ultra-strong photovoltaic pipe pile materials was prepared, which solved the problem of poor plasticization effect of water reducing agents in the prior art. It significantly improves the strength and durability of concrete, achieving cost reduction and efficiency enhancement effect.
Patent Information
- Application Number
- CN202411166915.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
UHPC ultra-strong photovoltaic pipe pile materials require extremely high strength and durability, but the plasticization effect of existing water reducing agents is poor, and it cannot effectively control slump loss and water leakage phenomenon, and cannot improve the strength and durability of concrete.
Using modified polycarboxylic acid water reducing agent, a composite water reducing agent is prepared by introducing lignin and other compounds such as alcohol amines, rosin thermal polymers, silicone defoaming agents, etc., to improve its dispersion performance and stability. , enhance compatibility with cement particles and optimize the microstructure of concrete.
It effectively improves the strength, durability, permeability and frost resistance of concrete, improves slump and water excretion rate, reduces production costs, achieves cost reduction and efficiency improvement, and improves the overall performance of UHPC materials.
Smart Images

Figure BDA0005008133790000071 
Figure BDA0005008133790000081 
Figure BDA0005008133790000082
Abstract
Description
Technical Field
[0001] The invention relates to the field of water reducing agents, and in particular to a composite water reducing agent for UHPC ultra-strong photovoltaic pipe pile materials and a preparation method thereof. Background Art
[0002] In today's construction and engineering fields, with the continuous advancement of technology and increasingly stringent requirements for material performance, the research and development of new high-performance materials has become the key to promoting the development of the industry. Ultra-High Performance Concrete (UHPC), as an innovative material with excellent performance, is gradually showing great application potential in various important structures, including the field of photovoltaic pipe piles.
[0003] UHPC has ultra-high strength, excellent durability, excellent impermeability and good working performance, which makes it an ideal choice for building high-quality, long-life infrastructure. However, to achieve these superior properties of UHPC, extremely high requirements are placed on its mix design and the selection of admixtures. Among the many admixtures, water reducer plays a vital role. It can significantly reduce the water-binder ratio of concrete, improve the fluidity and working performance of concrete, and have an important impact on the strength and durability of concrete.
[0004] With the rapid development of the photovoltaic industry, photovoltaic pipe piles, as important structural components for supporting and fixing photovoltaic equipment, need to have higher strength, better weather resistance and more stable performance. Traditional concrete pipe piles often have some limitations when facing complex environmental conditions and long-term use requirements, such as insufficient strength, poor durability, and easy cracking. The emergence of UHPC provides a possibility to solve these problems, but it also poses new challenges to material preparation and performance optimization.
[0005] In the preparation process of UHPC, the role of water reducer is not only to reduce water consumption and improve fluidity, but more importantly to achieve efficient dispersion of cement particles and optimize the microstructure of cement paste, thereby improving the overall performance of concrete. The effect of traditional water reducers in UHPC systems is often unsatisfactory and cannot meet its requirements for high performance. Therefore, the development of composite water reducers specifically suitable for UHPC ultra-strong photovoltaic pipe pile materials has become a hot topic in current research.
[0006] As a new generation of high-performance water-reducing agent, polycarboxylate water-reducing agent has the advantages of high water-reducing rate, good slump retention performance, and environmental protection, and has been widely used in the concrete industry. However, in the UHPC system, the use of polycarboxylate water-reducing agent alone may have some shortcomings, such as compatibility issues with other materials and poor adaptability to certain cement varieties. In order to further improve the performance of polycarboxylate water-reducing agent, modifying it has become an effective solution. By introducing specific functional groups or changing the molecular structure, the dispersion performance of polycarboxylate water-reducing agent can be improved, and its compatibility with other materials can be enhanced, so as to better meet the requirements of UHPC.
[0007] Lignin is a natural polymer compound that is widely present in plant cell walls. It has abundant active groups, such as hydroxyl, carboxyl, phenolic hydroxyl, etc. Using lignin to modify polycarboxylate water reducer can not only reduce costs, but also improve the performance of water reducer by utilizing the active groups of lignin to interact with polycarboxylate water reducer molecules. Lignin-modified polycarboxylate water reducer shows better performance in slump and water bleeding rate, which can effectively improve the working performance of UHPC, reduce the segregation and water bleeding of concrete, and make concrete more uniform and dense.
[0008] With the continuous advancement of science and technology and the pursuit of sustainable development, the research on composite water reducers for UHPC ultra-strong photovoltaic pipe pile materials will continue to deepen in the future. For example, further optimize the molecular structure and performance of water reducers, develop more environmentally friendly and efficient raw materials, explore new preparation processes and application technologies, etc. It is believed that with continuous innovation and efforts, UHPC ultra-strong photovoltaic pipe pile materials will play a more important role in promoting the development of the photovoltaic industry and infrastructure construction.
[0009] In response to the problems existing in the prior art, this application aims to solve the problems that UHPC ultra-strong photovoltaic pipe pile materials are required to have extremely high strength and durability, and the water reducer in the prior art has poor plasticizing effect, cannot effectively control slump loss and water seepage, and cannot improve the strength of UHPC ultra-strong photovoltaic pipe pile materials. Summary of the invention
[0010] Purpose of the invention: The purpose of the present invention is to provide a composite water reducer for UHPC ultra-strong photovoltaic pipe pile materials and a preparation method thereof, so as to solve the problems that UHPC ultra-strong photovoltaic pipe pile materials are required to have extremely high strength and durability, the water reducer in the prior art has poor plasticizing effect, cannot effectively control slump loss and water bleeding, and cannot improve the strength of UHPC ultra-strong photovoltaic pipe pile materials.
[0011] The technical solution of the present invention:
[0012] The invention provides a composite water reducer for UHPC super-strong photovoltaic pipe pile materials, characterized in that the raw materials of the composite water reducer for UHPC super-strong photovoltaic pipe pile materials include, by weight, 22 to 36 parts of modified polycarboxylic acid water reducer, 10 to 15 parts of alcohol amine compounds, 6 to 8 parts of rosin thermal polymers, 0.5 to 1 part of silicone defoamer, 2 to 8 parts of antifreeze, 5 to 10 parts of inorganic salts, and 30 to 65 parts of deionized water.
[0013] Furthermore, the raw materials for preparing the modified polycarboxylic acid water-reducing agent include: modified lignin polyoxyethylene ether, isodecyl alcohol polyoxyethylene ether, ammonium persulfate, and acrylamide.
[0014] Furthermore, the preparation method of the modified lignin polyoxyethylene ether comprises the following steps:
[0015] S1: weigh isodecyl alcohol polyoxyethylene ether in a flask, heat to 50-60°C until completely melted, add boron trifluoride etherate, then drop methyl epichlorohydrin, react at 50-60°C for 1-2 hours after the dropwise addition, to obtain a polymer;
[0016] S2: adding the polymer prepared in step S1 to a lignin solution with a pH of 12 to 13, heating to 70 to 80° C., and reacting for 2 to 3 hours;
[0017] S3: After the reaction is completed, the reaction solution is cooled and poured into ethanol to separate the solid and liquid and remove impurities. Then, isopropanol is added to precipitate and filter to obtain modified lignin polyoxyethylene ether.
[0018] Furthermore, the mass fraction of the lignin solution is 25-40%.
[0019] Furthermore, the mass ratio of the isodecyl alcohol polyoxyethylene ether to the lignin solution is 1:1 to 2.5.
[0020] Furthermore, the preparation method of the modified polycarboxylate water-reducing agent comprises the following steps:
[0021] S1: Weigh modified lignin polyoxyethylene ether and isodecyl alcohol polyoxyethylene ether into a three-necked flask, add a certain amount of deionized water to make a solution, and heat and stir to 70-80°C;
[0022] S2: adding ammonium persulfate in step S1, and then simultaneously dropping acrylamide, ascorbic acid, and mercaptoethanol aqueous solution, dropping acrylamide for 2 to 2.5 hours, dropping ascorbic acid and mercaptoethanol aqueous solution for 2.5 to 3 hours, and after the dropping is completed, keeping warm for 1 to 1.5 hours;
[0023] S3: After the heat preservation is completed, the reaction solution is adjusted to a pH of 6.5 to 7.5 with a NaOH solution to obtain a modified polycarboxylic acid water-reducing agent.
[0024] Furthermore, the mass ratio of the modified lignin polyoxyethylene ether, isodecyl alcohol polyoxyethylene ether, and acrylamide is 1:5-10:12-18;
[0025] Furthermore, the mass of the ammonium persulfate is 1.8-2.5% of the total mass of the modified lignin polyoxyethylene ether, isodecanol polyoxyethylene ether and acrylamide.
[0026] Furthermore, the rosin thermal polymer is a mixture of one or more of sodium rosin acid thermal polymer, rosin pentaerythritol ester thermal polymer, rosin styrene thermal polymer, and rosin maleic anhydride thermal polymer.
[0027] The present invention also provides a method for preparing a composite water reducing agent for UHPC ultra-strong photovoltaic pipe pile material, which is characterized by comprising the following steps:
[0028] Step (1): weighing a modified polycarboxylic acid water-reducing agent, an alcohol amine compound, a rosin thermal polymer, an organosilicon defoaming agent, an antifreeze agent, an inorganic salt, and deionized water for later use;
[0029] Step (2): add an appropriate amount of deionized water into the reaction container, turn on the stirring device, slowly add the modified polycarboxylate water reducer, and stir to fully dissolve it;
[0030] Step (3): then add the alcohol amine compound, rosin thermal polymer, silicone defoamer, antifreeze agent, and inorganic salt to step (2) in sequence, and continue stirring for a period of time to allow the components to fully mix and react to obtain a composite water reducer for UHPC ultra-strong photovoltaic pipe pile material.
[0031] Furthermore, the model of the rosin thermal polymer is a mixture of one or more of QS-03, TH-02, and PC-01.
[0032] Furthermore, the alcoholamine compound is a mixture of one or more of diethanol monoisopropanolamine, methyldiethanolamine, and triisopropanolamine.
[0033] Furthermore, the organosilicon defoamer is a mixture of one or more of acp0001 defoamer, s-101 organosilicon defoamer, and aq-305 organosilicon defoamer.
[0034] Furthermore, the antifreeze agent is a mixture of one or more of calcium chloride and ethylene glycol.
[0035] Furthermore, the inorganic salt is a mixture of one or more of sodium sulfate, sodium nitrate and sodium chloride.
[0036] The anionic groups (such as carboxyl, sulfonic acid, etc.) in the polycarboxylate water-reducing agent molecules will be adsorbed on the surface of cement particles, making the surface of cement particles carry the same negative charge. Since the same charges repel each other, electrostatic repulsion is generated, which prevents the agglomeration of cement particles and makes the cement particles dispersed more evenly. The introduction of lignin enhances this electrostatic repulsion effect, changes the charge distribution, and further improves the dispersion performance.
[0037] The main chain and side chain of the polycarboxylate water-reducing agent molecule form a thick adsorption layer on the surface of cement particles, which produces a steric hindrance effect and hinders the cement particles from approaching and agglomerating each other. The modification of lignin adjusts the length and structure of the molecular chain, optimizes the effect of steric hindrance, and enhances the dispersing and stabilizing effect on cement particles. Lignin contains some functional groups, such as hydroxyl and phenolic hydroxyl, which can react with metal ions (such as calcium ions) in cement paste, reduce the components in cement paste that are conducive to agglomeration, and thus improve the dispersibility. Water-reducing agent can reduce the interfacial tension between cement particles and water, increase the wetting degree of cement particles, and make cement particles more easily dispersed in water; during the concrete mixing process, lignin-modified polycarboxylate water-reducing agent can quickly adsorb on the surface of cement particles, and through the synergistic effect of the above-mentioned multiple action mechanisms, effectively disperse cement particles, reduce water consumption, and improve the fluidity and working performance of concrete.
[0038] Improve the plasticizing effect of water reducers, improve slump and water seepage rate, enhance the stability and adaptability of water reducers, reduce production costs, and improve the environmental performance of water reducers. Traditional water reducers may not provide sufficient plasticizing effect, resulting in poor workability of concrete, affecting construction efficiency and product quality. As a renewable resource, lignin modified water reducers may have better environmental friendliness and reduce the impact on the environment. By improving the performance of water reducers, the active groups of lignin combined with polycarboxylate water reducers may help improve the microstructure of concrete, thereby improving its overall performance, and improving the impermeability and antifreeze performance of UHPC in photovoltaics. High-performance water reducers are often expensive. By modifying polycarboxylate water reducers with lignin, it helps to improve the long-term performance of concrete, including crack resistance and durability, achieve cost reduction and efficiency improvement, and make UHPC materials more economical and practical.
[0039] Beneficial effects:
[0040] The present invention provides a composite water reducer for a UHPC super-strong photovoltaic pipe pile material. The composite water reducer for a UHPC super-strong photovoltaic pipe pile material has a good plasticizing effect, can improve the slump and water bleeding rate, and enhances the stability and adaptability of the water reducer, thereby achieving the purpose of reducing costs and increasing efficiency. Therefore, the strength, durability, impermeability and frost resistance of concrete can be effectively enhanced, and the composite water reducer has a long-term application prospect. DETAILED DESCRIPTION
[0041] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.
[0042] Lignin was purchased from Jinan Shengquan Group Co., Ltd.; isodecyl alcohol polyoxyethylene ether was purchased from Shanghai McLean Biochemical Technology Co., Ltd.; polycarboxylic acid water reducer was purchased from Jiangsu Subot New Materials Co., Ltd.; sodium rosin acid thermal polymer, rosin styrene thermal polymer, and rosin maleic anhydride thermal polymer were purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.
[0043] Unless otherwise specified, other chemical reagents used in the present invention are of commercially available analytical grade.
[0044] Lignin solution preparation:
[0045] Dimethyl sulfoxide and deionized water were prepared into a mixed solvent in a ratio of 8:2, and then 42.86 g of lignin was weighed and added into the above 100 mL mixed solvent, and stirred with a magnetic stirrer to fully dissolve the lignin to obtain a lignin solution with a mass fraction of 30%; lignin solutions with mass fractions of 20%, 30%, and 50% were prepared respectively according to the above method.
[0046] Preparation of modified lignin polyoxyethylene ether A:
[0047] S1: Weigh 100 g of isodecyl alcohol polyoxyethylene ether into a flask, heat it at 60°C until it is completely melted, add 0.2 g of boron trifluoride ether, and then drop 5 g of methyl epichlorohydrin. After the dropwise addition, react at 60°C for 2 hours to obtain a polymer;
[0048] S2: adding 100 g of the polymer prepared in step S1 to 150 g of a 30% lignin solution with a pH of 13, heating to 80° C., and reacting for 2 hours;
[0049] S3: After the reaction is completed, cool the reaction solution and pour it into 100 mL of ethanol to separate the solid and liquid and remove impurities. Then, add 100 mL of isopropanol for precipitation and filter to obtain modified lignin polyoxyethylene ether A.
[0050] Preparation of modified lignin polyoxyethylene ether B:
[0051] The preparation method of the present invention is the same as that of the modified lignin polyoxyethylene ether A, and the components and contents used are basically the same, except that: the 150 g of lignin solution with a mass fraction of 30% in step S2 is replaced by 150 g of lignin solution with a mass fraction of 20%.
[0052] Preparation of modified lignin polyoxyethylene ether C:
[0053] This preparation is the same as the preparation method of modified lignin polyoxyethylene ether A, and the components and contents used are basically the same. The difference is that the 150g lignin solution with a mass fraction of 30% in step S2 is replaced by 150g lignin solution with a mass fraction of 50%.
[0054] Preparation of modified lignin polyoxyethylene ether D:
[0055] The preparation method of this invention is the same as that of the modified lignin polyoxyethylene ether A, and the components and contents used are basically the same, except that: the 150 g lignin solution with a mass fraction of 30% in step S2 is replaced by 80 g lignin solution with a mass fraction of 30%.
[0056] Preparation of modified polycarboxylate water reducer A:
[0057] S1: Weigh 10g of modified lignin polyoxyethylene ether A and 80g of isodecyl alcohol polyoxyethylene ether into a three-necked flask, add 50mL of deionized water to make a solution, and heat and stir to 70-80°C;
[0058] S2: Add 4.8 g of ammonium persulfate in step S1, then simultaneously dropwise add 150 g of acrylamide, 0.48 g of ascorbic acid, and 1.2 g of a mercaptoethanol aqueous solution. Add acrylamide for 2 hours, and add ascorbic acid and mercaptoethanol aqueous solution for 3 hours. After the addition is completed, keep warm for 1.5 hours.
[0059] S3: After the heat preservation is completed, the pH of the reaction solution is adjusted to 7 with a 30% by mass NaOH solution to obtain a modified polycarboxylic acid water reducer.
[0060] Preparation of modified polycarboxylate water reducer B:
[0061] The preparation method of this invention is the same as that of the modified polycarboxylate water-reducing agent A, and the components and contents used are basically the same, except that 4.8 g of ammonium persulfate in step S2 is replaced by 2.4 g of ammonium persulfate.
[0062] Preparation of modified polycarboxylate water reducer C:
[0063] The preparation method of this invention is the same as that of modified polycarboxylate water reducer A, and the components and contents used are basically the same. The difference is that: 10 g of modified lignin polyoxyethylene ether and 80 g of isodecyl alcohol polyoxyethylene ether in step S1 are replaced by 10 g of modified lignin polyoxyethylene ether and 30 g of isodecyl alcohol polyoxyethylene ether; 150 g of acrylamide in step S2 is replaced by 200 g of acrylamide.
[0064] Preparation of modified polycarboxylate water reducer D:
[0065] The preparation method of the present invention is the same as that of the modified polycarboxylate water reducer A, and the components and contents used are basically the same, except that the modified lignin polyoxyethylene ether A in step S1 is replaced by modified lignin polyoxyethylene ether B.
[0066] Preparation of modified polycarboxylate water reducer E:
[0067] The preparation method of the present invention is the same as that of the modified polycarboxylate water reducer A, and the components and contents used are basically the same, except that the modified lignin polyoxyethylene ether A in step S1 is replaced by modified lignin polyoxyethylene ether C.
[0068] Preparation of modified polycarboxylate water reducer F:
[0069] The preparation method of the present invention is the same as that of the modified polycarboxylate water reducer A, and the components and contents used are basically the same, except that the modified lignin polyoxyethylene ether A in step S1 is replaced by modified lignin polyoxyethylene ether D.
[0070] Preparation method of composite water reducing agent for UHPC ultra-strong photovoltaic pipe pile material:
[0071] Step (1): weighing a modified polycarboxylic acid water-reducing agent, an alcohol amine compound, a rosin thermal polymer, an organosilicon defoaming agent, an antifreeze agent, an inorganic salt, and deionized water for later use;
[0072] Step (2): first add deionized water into the reaction container, turn on the stirring device, slowly add the modified polycarboxylate water reducer, and stir to fully dissolve it;
[0073] Step (3): then add the alcohol amine compound, rosin thermal polymer, silicone defoamer, antifreeze agent, and inorganic salt to step (2) in sequence, and continue stirring for a period of time to allow the components to fully mix and react to obtain a composite water reducer for UHPC ultra-strong photovoltaic pipe pile material.
[0074] Examples 1 to 8
[0075] The composite water reducer for UHPC ultra-strong photovoltaic pipe pile material is prepared according to the preparation method of the composite water reducer for UHPC ultra-strong photovoltaic pipe pile material. Table 1 is the ingredient list of the composite water reducer for UHPC ultra-strong photovoltaic pipe pile material of Examples 1 to 8.
[0076] Table 1 Ingredients of composite water reducing agent for UHPC ultra-strong photovoltaic pipe pile materials in Examples 1 to 8
[0077]
[0078] Comparative Examples 1 to 3:
[0079] The composite water reducer for UHPC ultra-strong photovoltaic pipe pile material is prepared according to the preparation method of the composite water reducer for UHPC ultra-strong photovoltaic pipe pile material. Table 2 is the ingredient list of the composite water reducer for UHPC ultra-strong photovoltaic pipe pile material of Comparative Examples 1 to 3.
[0080] Table 2 Ingredients of composite water reducing agent for UHPC ultra-strong photovoltaic pipe pile materials in comparative examples 1 to 3
[0081]
[0082]
[0083] Performance Test:
[0084] First, prepare ordinary Portland cement and water, and make a reference slurry with an ordinary Portland cement to water-cement ratio of 8:2. Then, at the same water-cement ratio, add 2% of the mass of ordinary Portland cement in the composite water-reducing agent for UHPC ultra-strong photovoltaic pipe pile materials prepared in Examples 1 to 8 and Comparative Examples 1 to 3, and stir again to make a test slurry. According to the standards GB / T50080-2016 "Standard for Test Methods of Ordinary Concrete Mixtures Performance" and GB / T 8077-2012 "Test Methods for Homogeneity of Concrete Admixtures", the following characteristics are tested:
[0085] 1. Plasticizing effect: The net slurry fluidity method measures the fluidity of the reference net slurry and the test net slurry within a specified time. The increase in fluidity reflects the plasticizing effect of the water reducer.
[0086] 2. Slump: Test the initial slump of the benchmark pure paste, add a predetermined amount of water reducer, stir again and measure the slump. The increase in slump reflects the effect of the water reducer in improving the slump.
[0087] 3. Water seepage rate: For the normal pressure water seepage rate test, concrete is mixed according to the specified mix ratio, and the concrete mixture is loaded into a 5L covered cylinder at a time. It is vibrated on a vibration table until slurry appears on the surface, and then smoothed with a spatula, and then covered and allowed to stand. From the beginning of the standing time, the water seepage is sucked out every 10 minutes for the first 60 minutes; after 60 minutes, the water seepage is sucked out every 30 minutes until it is considered that there is no more water seepage. The formula for calculating the water seepage rate is: Water seepage rate = (total water seepage / total water content in the concrete mixture × 100%).
[0088] Table 3: Performance test results
[0089] The measured fluidity of the benchmark pure slurry is 180mm, the slump is 90mm, and the water bleeding rate is 3.3%;
[0090]
[0091]
[0092] It can be seen from Table 3 that the composite water reducing agent for UHPC ultra-strong photovoltaic pipe pile material prepared by the present invention can effectively improve the slump and water bleeding rate, and has a good plasticizing effect. Specifically, from the comparison between Example 4 and Example 3, it can be seen that when preparing the modified polycarboxylic acid water-reducing agent, too little ammonium persulfate content will cause the prepared composite water-reducing agent to have poor plasticizing effect on concrete, poor slump and water bleeding rate; from the comparison between Example 5 and Example 3, it can be seen that when preparing the modified polycarboxylic acid water-reducing agent, the unreasonable mass ratio of modified lignin polyoxyethylene ether, isodecyl alcohol polyoxyethylene ether and acrylamide will cause the prepared composite water-reducing agent to have poor plasticizing effect on concrete, poor slump and water bleeding rate; from the comparison between Examples 6 to 7 and Example 3, it can be seen that when preparing the modified lignin polyoxyethylene ether, the mass concentration of the lignin solution is too large or too small, which will affect the prepared composite water-reducing agent to have poor plasticizing effect on concrete and poor water bleeding rate; from the comparison between Example 8 and Example 3, it can be seen that when preparing the modified lignin polyoxyethylene ether, the unreasonable mass ratio of isodecyl alcohol polyoxyethylene ether to the lignin solution will cause the prepared composite water-reducing agent to have poor plasticizing effect on concrete and poor water bleeding rate;
[0093] From the comparison between Comparative Example 1 and Example 3, it can be seen that when the modified polycarboxylate water-reducing agent is not added, the plasticizing effect of the prepared composite water-reducing agent on the concrete deteriorates, and the slump and water bleeding rate deteriorate, and the standard is not met; from the comparison between Comparative Example 2 and Example 3, it can be seen that when the modified polycarboxylate water-reducing agent is replaced with the ordinary polycarboxylate water-reducing agent, the plasticizing effect, slump and water bleeding rate of the prepared composite water-reducing agent for adding UHPC super-strong photovoltaic pipe pile material on the concrete are not as good as those in the embodiment; from the comparison between Comparative Example 3 and Example 2, it can be seen that when the rosin thermopolymer is not added, the plasticizing effect, slump and water bleeding rate of the prepared composite water-reducing agent for adding UHPC super-strong photovoltaic pipe pile material on the concrete deteriorate, and the expected effect is not achieved.
[0094] The present invention can also have many other embodiments. Without departing from the spirit and essence of the present invention, those skilled in the art can make various corresponding changes and modifications based on the present invention, but these corresponding changes and modifications should all fall within the scope of protection of the claims attached to the present invention.
Claims
1. A composite water reducing agent for UHPC ultra-strong photovoltaic pipe pile material, characterized in that: The raw materials of the composite water reducer for UHPC ultra-strong photovoltaic pipe pile material include, by weight: 22 to 36 parts of modified polycarboxylic acid water reducer, 10 to 15 parts of alcohol amine compounds, 6 to 8 parts of rosin thermal polymer, 0.5 to 1 part of silicone defoamer, 2 to 8 parts of antifreeze, 5 to 10 parts of inorganic salt, and 30 to 65 parts of deionized water.
2. The composite water reducing agent for UHPC ultra-strong photovoltaic pipe pile material according to claim 1, characterized in that: The raw materials for preparing the modified polycarboxylic acid water-reducing agent include: modified lignin polyoxyethylene ether, isodecyl alcohol polyoxyethylene ether, ammonium persulfate and acrylamide.
3. The composite water reducing agent for UHPC ultra-strong photovoltaic pipe pile material according to claim 2, characterized in that: The preparation method of the modified lignin polyoxyethylene ether comprises the following steps: S1: weigh isodecyl alcohol polyoxyethylene ether in a flask, heat to 50-60°C until completely melted, add boron trifluoride etherate, then drop methyl epichlorohydrin, react at 50-60°C for 1-2 hours after the dropwise addition, to obtain a polymer; S2: adding the polymer prepared in step S1 to a lignin solution with a pH of 12 to 13, heating to 70 to 80° C., and reacting for 2 to 3 hours; S3: After the reaction is completed, the reaction solution is cooled and poured into ethanol to separate the solid and liquid and remove impurities. Then, isopropanol is added to precipitate and filter to obtain modified lignin polyoxyethylene ether.
4. The composite water reducing agent for UHPC ultra-strong photovoltaic pipe pile material according to claim 3, characterized in that: The mass fraction of the lignin solution is 25-40%.
5. The composite water reducing agent for UHPC ultra-strong photovoltaic pipe pile material according to claim 3, characterized in that: The mass ratio of the isodecyl alcohol polyoxyethylene ether to the lignin solution is 1:1-2.
5.
6. The composite water reducing agent for UHPC ultra-strong photovoltaic pipe pile material according to claim 1, characterized in that: The preparation method of the modified polycarboxylate water-reducing agent comprises the following steps: S1: Weigh modified lignin polyoxyethylene ether and isodecyl alcohol polyoxyethylene ether into a three-necked flask, add a certain amount of deionized water to make a solution, and heat and stir to 70-80°C; S2: adding ammonium persulfate in step S1, and then simultaneously dropping acrylamide, ascorbic acid, and mercaptoethanol aqueous solution, dropping acrylamide for 2 to 2.5 hours, dropping ascorbic acid and mercaptoethanol aqueous solution for 2.5 to 3 hours, and after the dropping is completed, keeping warm for 1 to 1.5 hours; S3: After the heat preservation is completed, the reaction solution is adjusted to a pH of 6.5 to 7.5 with a NaOH solution to obtain a modified polycarboxylic acid water-reducing agent.
7. The composite water reducing agent for UHPC ultra-strong photovoltaic pipe pile material according to any one of claims 2 or 6, characterized in that: The mass ratio of the modified lignin polyoxyethylene ether, isodecyl alcohol polyoxyethylene ether and acrylamide is 1:5-10:12-18.
8. The composite water reducing agent for UHPC ultra-strong photovoltaic pipe pile material according to any one of claims 2 or 6, characterized in that: The mass of the ammonium persulfate is 1.8-2.5% of the total mass of the modified lignin polyoxyethylene ether, isodecanol polyoxyethylene ether and acrylamide.
9. The composite water reducing agent for UHPC ultra-strong photovoltaic pipe pile material according to claim 1, characterized in that: The rosin thermal polymer is a mixture of one or more of sodium rosin acid thermal polymer, rosin pentaerythritol ester thermal polymer, rosin styrene thermal polymer and rosin maleic anhydride thermal polymer.
10. The method for preparing the composite water reducing agent for UHPC ultra-strong photovoltaic pipe pile material according to any one of claims 1 to 9, characterized in that: The following steps are involved: Step (1): weighing a modified polycarboxylic acid water-reducing agent, an alcohol amine compound, a rosin thermal polymer, an organosilicon defoaming agent, an antifreeze agent, an inorganic salt, and deionized water for later use; Step (2): add an appropriate amount of deionized water into the reaction container, turn on the stirring device, slowly add the modified polycarboxylate water reducer, and stir to fully dissolve it; Step (3): then add the alcohol amine compound, rosin thermal polymer, silicone defoamer, antifreeze agent, and inorganic salt to step (2) in sequence, and continue stirring for a period of time to allow the components to fully mix and react to obtain a composite water reducer for UHPC ultra-strong photovoltaic pipe pile material.