Preparation process of porous cement-based material compatible with electromagnetic shielding and infrared protection
By using spherical highly water-absorbing organic polymer modified by magnetic nanomaterials in cement-based materials to form small pore structures, the mechanical properties and infrared detection problems of traditional electromagnetic shielding materials are solved, and better electromagnetic shielding and stealth effects are achieved.
Patent Information
- Application Number
- CN202411228512.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-03
AI Technical Summary
Traditional composite cement-based electromagnetic shielding materials have reduced mechanical properties due to the high density of wave absorbing materials and the cohesive damage to cement stones, and are easily detected by infrared thermal imaging systems, affecting the confidentiality of the anti-electromagnetic system.
Spherical highly water-absorbing organic polymer modified with magnetic nanomaterials forms a small pore structure in cement-based materials, increasing the reflection and scattering of electromagnetic waves, reducing the generation and transfer of heat, and reducing infrared detectability.
It achieves good electromagnetic shielding effect and stealth performance, avoids the decline in mechanical properties of traditional materials and the risks of infrared detection, and enhances the confidentiality of military facilities.
Smart Images

Figure CN119038929A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electromagnetic shielding cement-based materials, and in particular to a preparation process of a porous cement-based material that is electromagnetic shielding and compatible with infrared protection. Background Art
[0002] Electromagnetic waves can cause electromagnetic interference, which not only seriously threatens the normal operation of equipment and the stability of communication systems, but can also be used to detect and locate equipment, making military infrastructure and strategic target buildings face great risks of electromagnetic leakage and the resulting information leakage, which will directly endanger the country's political, economic and military security. The traditional composite cement-based electromagnetic shielding system absorbs electromagnetic waves by adding absorbing materials such as graphite and carbon powder. Although it has a certain electromagnetic shielding effect, the high density of the absorbing material itself can easily lead to an increase in the bulk density of components or load-bearing structures. In addition, the absorbing material will also destroy the cohesion of the cement stone, deteriorate the pore structure, and lead to reduced mechanical properties. In addition, the heat generated by the absorption of electromagnetic waves by this type of traditional composite cement-based electromagnetic shielding material is very easy to be detected by the infrared thermal imaging system, which seriously affects the confidentiality of the anti-electromagnetic system. Summary of the invention
[0003] In view of the above problems, the present invention provides a preparation process of a porous cement-based material compatible with electromagnetic shielding and infrared protection, which forms a special pore structure inside the cement-based material by adding a highly water-absorbent organic polymer modified by magnetic nanomaterials, which not only has a good electromagnetic shielding effect, but also significantly reduces the heat generated during the electromagnetic wave loss process, reduces infrared detectability, and makes the cement-based material of the present invention have a better stealth effect. Specifically, the technical solution of the present invention is as follows.
[0004] A preparation process of a porous cement-based material compatible with electromagnetic shielding and infrared protection, comprising the following steps: (1) The dispersion medium and the surfactant are mixed and heated and stirred to obtain an oil phase for later use.
[0005] (2) Add the hydrophilic polymer monomer into water and stir until fully dissolved. Then add the initiator and the cross-linking agent and stir evenly to obtain the aqueous phase.
[0006] (3) adding the aqueous phase to the oil phase and stirring until dispersed, and then carrying out a polymerization reaction under heating and stirring conditions, and finally separating the solid product, washing to obtain a spherical highly water-absorbent organic polymer for standby use.
[0007] (4) adding the highly spherical and highly absorbent organic polymer to a liquid phase for soaking, then adding the absorbent gel to a magnetic nanoparticle dispersion medium containing a surfactant, stirring the reaction, separating the solid product, and washing the solid product to obtain a core-shell structured magnetic nanoparticle-modified highly absorbent organic polymer.
[0008] (5) The modified highly water-absorbent organic polymer is added to cement-based materials to prepare slurry and then cured to obtain a porous cement-based material.
[0009] Furthermore, in step (1), the mass ratio of the dispersion medium to the surfactant is 1-5:0.025-0.075. Optionally, the dispersion medium includes at least one of n-heptane, isooctane, cyclohexane, n-hexane, 2-methylpentane, etc. The surfactant includes at least one of silicone oil, sodium dodecyl sulfate, sodium octadecyl sulfate, Span 60, Span 80, Tween 20, Tween 60, Tween 80, etc.
[0010] Furthermore, in step (1), the heating temperature is 30-60° C., and the stirring time is 10-30 min.
[0011] Furthermore, in step (2), the mass ratio of the hydrophilic polymer monomer to water is 0.5-1:15-40. Optionally, the hydrophilic polymer monomer includes at least one of acrylic acid, methacrylic acid, acrylamide, 2-acrylamide-2-methylpropanesulfonic acid, sodium vinyl sulfonate, etc.
[0012] Furthermore, in step (2), the mass ratio of the hydrophilic polymer monomer, the initiator, and the cross-linking agent is 0.5-1: 0.025-0.075: 0.005-0.01.
[0013] Furthermore, in step (2), the initiator includes at least one of potassium persulfate, sodium persulfate, ammonium persulfate, hydrogen peroxide, tert-butyl hydroperoxide, tert-butyl peroxy-2-ethylhexanoate, azobisisobutyronitrile, etc.
[0014] Furthermore, in step (2), the cross-linking agent includes at least one of vinylmethyloxyvinylsilane, divinylbenzene, vinyl acrylic acid, N,N'-methylenebisacrylamide, methyl trimethacrylate, etc.
[0015] Furthermore, in step (2), the stirring time is 10 to 30 minutes.
[0016] Furthermore, in step (3), the mass ratio of the water phase to the oil phase is 1:2 to 8. Optionally, the water phase is added to the oil phase and stirred for 10 to 30 minutes.
[0017] Furthermore, in step (3), the heating temperature is 50-100° C., and the stirring time is 1-3 hours. Optionally, the solid product is washed with any one of anhydrous ethanol, isopropanol, dichloromethane, ether, etc.
[0018] Furthermore, in step (4), the mass ratio of the spherical highly absorbent organic polymer to the liquid phase is 0.5-1.1:1-5. Optionally, the liquid phase includes any one of ammonia water, white vinegar solution, water, etc. Optionally, the mass fraction of the ammonia water or white vinegar solution is 10-30%.
[0019] Furthermore, in step (4), the soaking time is 12 to 24 hours.
[0020] Furthermore, in step (4), the volume ratio of the water-absorbing gel to the magnetic nanoparticle dispersion containing a surfactant is 1:3-8. The mass ratio of the magnetic nanoparticles, the surfactant, and the dispersion medium is 1:0.05-0.3:2-6. Optionally, the surfactant and the dispersion medium are the same as above.
[0021] Furthermore, the magnetic nanoparticle dispersion containing a surfactant is prepared by the following method: the magnetic nanoparticles are first vacuum dried and activated for 2-8 hours, and then dispersed in the dispersion medium for ultrasonic treatment for 10-40 minutes. After completion, the surfactant is added, and then heated to 50-80° C. and stirred for 10-30 minutes.
[0022] Furthermore, in step (4), the magnetic nanoparticles include at least one of nano-Fe3O4, nano-cobalt powder, nano-nickel powder, etc. Optionally, the particle size of the magnetic nanoparticles is 20-90 nm.
[0023] Furthermore, in step (4), the stirring reaction time is 1 to 3 hours. The magnetic nanomaterial uses a large number of hydroxyl groups on its surface to chemically bond with the hydroxyl groups on the surface of the spherical highly water-absorbent organic polymer, so that the magnetic nanomaterial is uniformly coated on the surface of the organic polymer to form a core-shell structure. Optionally, in step (4), any one of anhydrous ethanol, isopropanol, dichloromethane, ether, etc. is used to wash the solid product.
[0024] Furthermore, in step (5), the magnetic nanoparticle-modified highly water-absorbent organic polymer accounts for 5-20% of the mass of the cement-based material.
[0025] Compared with the prior art, the technical solution of the present invention has at least the following beneficial effects: The present invention first prepares a spherical highly water-absorbent organic polymer, and then loads magnetic nanoparticles on the surface of the polymer to form a magnetic nanoparticle-modified highly water-absorbent organic polymer with a spherical core-shell structure. When such an electromagnetic shielding material is used to prepare a cement-based material. First, in the cement hydration stage, the spherical highly water-absorbent organic polymer absorbs the mixing water in the cement material to form a gel ball. As the hydration reaction continues, the water-absorbent gel ball gradually releases water, ensuring that the later hydration reaction of the cement can be fully carried out, while maintaining the relative humidity inside the cement-based material, reducing shrinkage cracking caused by self-drying, and alleviating the adverse effects on the mechanical strength of the cement-based material. In the above-mentioned cement hydration and hardening process, the bonding and anchoring effect formed by the gel product and the magnetic nanoparticles on the surface of the gel ball separates the gel ball and the magnetic nanoparticles, thereby transferring the magnetic nanoparticles on the surface of the spherical highly water-absorbent organic polymer to the surface of the small pores, forming a special structure in which the surface of the small pores is covered with magnetic nanoparticles (refer to the attached figure of the specification). Figure 1 ).
[0026] When the cement-based material with the above-mentioned special structure is interfered by electromagnetic waves, firstly, the spherical holes can increase the number of reflections and scatterings of electromagnetic waves, increase the transmission path of electromagnetic waves, and the magnetic nanoparticles evenly distributed on the surface of the holes absorb electromagnetic waves, so that the electromagnetic waves are effectively lost. When electromagnetic waves are absorbed and converted into heat energy, due to the large specific surface area of magnetic nanomaterials, they can absorb the heat more fully at the microscopic level, and the presence of spherical holes prevents the heat from being immediately transferred to the outside of the material, but is stored in these tiny cavities to achieve the slow release of heat energy. This ensures that the temperature change of the material will not be large when it plays an electromagnetic shielding role, reduces the infrared detectability of the material, enhances the concealment of the material, and can play a better role in confidentiality for military facilities.
[0027] In addition, the present invention uses the spherical highly absorbent organic polymer as a carrier to evenly distribute the easily agglomerated magnetic nanoparticles into the cement-based material, thereby maximizing the electromagnetic shielding effect, while also avoiding the problem of increased infrared detectability of the region due to the agglomeration of magnetic nanoparticles, which results in a large amount of electromagnetic waves and heat consumed in the region. Compared with the traditional method of directly adding magnetic nanomaterials to cement-based materials to achieve electromagnetic shielding (see the attached drawings of the specification), Figure 2), the porous cement-based material of the present invention not only has better electromagnetic shielding ability and avoids being penetrated by electromagnetic waves, but also overcomes the problem that traditional electromagnetic shielding cement materials are easily detected by infrared. This is because traditional electromagnetic shielding cement materials mainly rely on the absorption of electromagnetic waves by magnetic nanomaterials distributed therein to achieve electromagnetic shielding function, but this absorption will cause the generated heat to accumulate in the wave absorption area, and the aggregation of magnetic nanomaterials will lead to concentrated absorption and concentrated heat generation, which makes it easier for the heat in the cement-based material to be transferred outward, thereby causing the surface temperature of the cement material to increase significantly and be easily detected by infrared. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0029] Figure 1 The schematic diagram of the porous cement-based material for electromagnetic shielding and infrared protection of the present invention; Figure 2 This is the principle diagram of the traditional method of directly adding magnetic nanomaterials into cement-based materials to achieve electromagnetic shielding; Figure 3 This is a sample of a spherical magnetic nanoparticle-modified highly water-absorbent organic polymer prepared in Example 1 below; Figure 4 The SEM image of the spherical magnetic nanoparticles modified highly water-absorbent organic polymer prepared in Example 1 below. DETAILED DESCRIPTION
[0030] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples without specifying specific conditions are usually carried out under conventional conditions or under conditions recommended by the manufacturer.
[0031] Unless otherwise defined, all professional and scientific terms used in the present invention have the same meanings as those familiar to those skilled in the art. The reagents or raw materials used in the present invention can be purchased through conventional channels. Unless otherwise specified, the reagents or raw materials used in the present invention are used in a conventional manner in the art or in accordance with the product instructions.
[0032] In addition, any method and material similar or equivalent to the described content can be applied to the method of the present invention. The technical solution of the present invention is further described in conjunction with the accompanying drawings and specific embodiments.
[0033] Example 1 A preparation process of a porous cement-based material compatible with electromagnetic shielding and infrared protection, comprising the following steps: (1) The dispersion medium (cyclohexane) and the surfactant (silicone oil) were mixed in a mass ratio of 3:0.04, heated to 60°C, and stirred for 10 minutes to obtain an oil phase for use.
[0034] (2) The hydrophilic polymer monomer (acrylic acid) and water were mixed in a mass ratio of 1:40 and magnetically stirred for 25 minutes to fully dissolve the polymer monomer. Then, an initiator (potassium persulfate) and a cross-linking agent (methyl trimethacrylate) were added and stirred for 20 minutes to obtain an aqueous phase for use. The mass ratio of the hydrophilic polymer monomer, the initiator, and the cross-linking agent was 1:0.075:0.008.
[0035] (3) The aqueous phase of step (2) and the oil phase of step (1) are mixed in a mass ratio of 1:5, stirred for 30 minutes, and then heated to 70° C. and stirred at this temperature for 2 hours to carry out polymerization reaction. After completion, the solid product is separated by filtration, washed with anhydrous ethanol and air-dried to obtain a spherical highly absorbent organic polymer for later use.
[0036] (4) Magnetic nanoparticles (Fe3O4 with a particle size of 20-90 nm) were vacuum dried and activated at 100°C for 5 h, then added to a dispersion medium (cyclohexane) and ultrasonicated for 20 min, then a surfactant (silicone oil) was added and heated to 70°C and stirred at this temperature for 15 min to obtain a dispersion for use. The mass ratio of the magnetic nanoparticles, surfactant, and dispersion medium was 1:0.1:4.
[0037] (5) The spherical highly absorbent organic polymer is added to 10% ammonia water and soaked for 24 hours, and the mass ratio of the two is 1:2.5. Then the obtained gel material is added to the dispersion (the volume ratio of the two is 1:4) and stirred for 1.5 hours. After completion, the solid product is separated by filtration, washed with anhydrous ethanol and dried to obtain a spherical core-shell structure magnetic nanoparticle modified highly absorbent organic polymer (such as Figure 3 and Figure 4 as shown), for standby use.
[0038] (6) 10% by weight of the spherical core-shell structured magnetic nanoparticle-modified highly absorbent organic polymer is added to 42.5% ordinary silica cement, and then clean water is added according to a water-cement ratio of 0.4 and stirred at 300 rpm for 2 min. The obtained slurry is poured into a mold and naturally cured for 24 h. After demolding, it is placed in a standard curing room and continued to be cured until the 28th day to obtain a porous cement-based material.
[0039] The reflectivity was measured by sweeping the frequency using the bow method, and the test frequency range was between 2GHz and 18GHz. At a wave frequency of 2.56 GHz, the reflectivity of the porous cement-based material of this embodiment to electromagnetic waves was -15.34dB. At a wave frequency of 17.28 GHz, the reflectivity of the porous cement-based material to electromagnetic waves was -10.46dB. Using an infrared thermal imager, it was measured that the temperature change of the porous cement-based material of this embodiment within 1 hour after absorbing electromagnetic waves was 1.5°C. Using a universal testing machine, it was measured that the 28d compressive strength of the porous cement-based material of this embodiment was 50.6MPa.
[0040] Example 2 A preparation process of a porous cement-based material compatible with electromagnetic shielding and infrared protection, comprising the following steps: (1) The dispersion medium (n-hexane) and the surfactant (sodium dodecyl sulfate) were mixed in a mass ratio of 1:0.025, heated to 40°C, and stirred for 20 minutes to obtain an oil phase for use.
[0041] (2) The hydrophilic polymer monomer (acrylamide) and water were mixed in a mass ratio of 0.6:25 and magnetically stirred for 10 minutes to fully dissolve the polymer monomer. Then, an initiator (ammonium persulfate) and a cross-linking agent (N,N'-methylenebisacrylamide) were added and stirred for 10 minutes to obtain an aqueous phase for use. The mass ratio of the hydrophilic polymer monomer, initiator, and cross-linking agent was 0.5:0.025:0.005.
[0042] (3) The aqueous phase of step (2) and the oil phase of step (1) are mixed in a mass ratio of 1:2, stirred for 10 minutes, and then heated to 50° C. and stirred at this temperature for 3 hours to carry out polymerization reaction. After completion, the solid product is separated by filtration, washed with isopropanol and dried to obtain a spherical highly absorbent organic polymer for later use.
[0043] (4) Activate the magnetic nanoparticles (nano cobalt powder with a particle size of 20-90 nm) by vacuum drying at 50°C for 8 h, then add them to a dispersion medium (n-hexane) and ultrasonicate for 10 min, then add a surfactant (sodium dodecyl sulfate) and heat to 50°C and stir at this temperature for 30 min to obtain a dispersion for use. The mass ratio of the magnetic nanoparticles, surfactant, and dispersion medium is 1:0.05:2.
[0044] (5) The spherical highly absorbent organic polymer is added to a 30% by mass white vinegar solution and soaked for 18 hours, with the mass ratio of the two being 0.5:1. The obtained gel material is then added to the dispersion (the volume ratio of the two being 1:3) and stirred for reaction for 1 hour. After completion, the solid product is separated by filtration, washed with isopropanol and air-dried to obtain a spherical core-shell structured magnetic nanoparticle-modified highly absorbent organic polymer for later use.
[0045] (6) Add 20% by weight of the magnetic nanoparticle-modified spherical highly absorbent organic polymer into 42.5% ordinary silica cement, then add clean water at a water-cement ratio of 0.5 and stir at a speed of 100 rpm for 5 minutes. Pour the obtained slurry into a mold and cure it naturally for 24 hours. After demolding, place it in a standard curing room and continue curing until the 28th day to obtain a porous cement-based material.
[0046] The reflectivity was measured by sweeping the frequency using the bow method, and the test frequency range was between 2GHz and 18GHz. At a wave frequency of 2.56 GHz, the reflectivity of the porous cement-based material of this embodiment to electromagnetic waves was -17.84dB. At a wave frequency of 17.28 GHz, the reflectivity of the porous cement-based material to electromagnetic waves was -11.75dB. Using an infrared thermal imager, it was measured that the temperature change of the porous cement-based material of this embodiment within 1 hour after absorbing electromagnetic waves was 1.3°C. Using a universal testing machine, it was measured that the 28d compressive strength of the porous cement-based material of this embodiment was 45.8MPa.
[0047] Example 3 A preparation process of a porous cement-based material compatible with electromagnetic shielding and infrared protection, comprising the following steps: (1) The dispersion medium (n-heptane) and the surfactant (Span 60) were mixed in a mass ratio of 1:0.075, heated to 30°C, and stirred for 30 minutes to obtain an oil phase for use.
[0048] (2) The hydrophilic polymer monomer (methacrylic acid) and water were mixed in a mass ratio of 0.5:15 and magnetically stirred for 10 minutes to fully dissolve the polymer monomer. Then, an initiator (azobisisobutyronitrile) and a cross-linking agent (divinylbenzene) were added and stirred for 30 minutes to obtain an aqueous phase for use. The mass ratio of the hydrophilic polymer monomer, initiator, and cross-linking agent was 0.75:0.06:0.01.
[0049] (3) The aqueous phase of step (2) and the oil phase of step (1) are mixed in a mass ratio of 1:8, stirred for 30 minutes, and then heated to 100° C. and stirred at this temperature for 1 hour to carry out polymerization reaction. After completion, the solid product is separated by filtration, washed with dichloromethane and air-dried to obtain a spherical highly absorbent organic polymer for later use.
[0050] (4) Activate the magnetic nanoparticles (nano nickel powder with a particle size of 20-90 nm) by vacuum drying at 80°C for 2 h, then add them to a dispersion medium (n-heptane) and ultrasonicate for 40 min, then add a surfactant (Span 60) and heat to 80°C and stir at this temperature for 10 min to obtain a dispersion for use. The mass ratio of the magnetic nanoparticles, surfactant, and dispersion medium is 1:0.3:6.
[0051] (5) The spherical highly absorbent organic polymer is added to water and soaked for 12 hours, and the mass ratio of the two is 1.5:5. Then the obtained gel material is added to the dispersion (the volume ratio of the two is 1:8) and stirred for 3 hours. After completion, the solid product is separated by filtration, washed with anhydrous ethanol and dried to obtain a core-shell magnetic nanoparticle modified spherical highly absorbent organic polymer for standby use.
[0052] (6) Add 5% by weight of the magnetic nanoparticle-modified spherical highly absorbent organic polymer into 42.5% ordinary silica cement, then add clean water at a water-cement ratio of 0.35 and stir at 200 rpm for 3 min. Pour the resulting slurry into a mold and cure it naturally for 24 h. After demolding, place it in a standard curing room and continue curing until the 28th day to obtain a porous cement-based material.
[0053] The reflectivity was measured by sweeping the frequency using the bow method, and the test frequency range was between 2GHz and 18GHz. At a wave frequency of 2.56 GHz, the reflectivity of the porous cement-based material of this embodiment to electromagnetic waves was -14.12dB. At a wave frequency of 17.28 GHz, the reflectivity of the porous cement-based material to electromagnetic waves was -9.15dB. Using an infrared thermal imager, it was measured that the temperature change of the porous cement-based material of this embodiment within 1 hour after absorbing electromagnetic waves was 2.2°C. Using a universal testing machine, it was measured that the 28d compressive strength of the porous cement-based material of this embodiment was 52.3MPa.
[0054] Example 4 A preparation process of an electromagnetic shielding porous cement-based material comprises the following steps: A mixture of 10% by weight of magnetic nanoparticles (Fe3O4 with a particle size of 20-90 nm) and spherical highly absorbent organic polymer (prepared in step (3) of the above Example 1) was added to 42.5% of ordinary silica cement (the mass ratio of the two was 1:0.784), and then clean water was added at a water-cement ratio of 0.4 and stirred at a speed of 300 rpm for 2 min. The obtained slurry was poured into a mold and naturally cured for 24 h. After demolding, it was placed in a standard curing room and continued to be cured until the 28th day, thereby obtaining a porous cement-based material.
[0055] The reflectivity was measured by sweeping the frequency using the bow method, and the test frequency range was between 2GHz and 18GHz. At a wave frequency of 2.56 GHz, the reflectivity of the porous cement-based material of this embodiment to electromagnetic waves was -7.2dB. At a wave frequency of 17.28GHz, the reflectivity of the porous cement-based material to electromagnetic waves was -3.5dB. Using an infrared thermal imager, it was measured that the temperature change of the porous cement-based material of this embodiment within 1 hour after absorbing electromagnetic waves was 2.5°C. Using a universal testing machine, it was measured that the 28d compressive strength of the porous cement-based material of this embodiment was 44.8MPa.
[0056] Example 5 A preparation process of an electromagnetic shielding porous cement-based material comprises the following steps: (1) Magnetic nanoparticles (nano cobalt powder with a particle size of 20-90 nm) were vacuum dried and activated at 50°C for 8 h, then added to a dispersion medium (n-hexane) and ultrasonicated for 10 min, then a surfactant (sodium dodecyl sulfate) was added and heated to 50°C and stirred at this temperature for 30 min to obtain a dispersion for use. The mass ratio of the magnetic nanoparticles, surfactant, and dispersion medium was 1:0.05:2.
[0057] (2) A commercially available water-absorbing resin (model B20, Renqiu Quanxing Chemical Co., Ltd.) was added to a 30% by mass white vinegar solution and soaked for 18 hours, with the mass ratio of the two being 0.5:1. The obtained gel material was then added to the dispersion (the volume ratio of the two being 1:3) and stirred for reaction for 1 hour. After completion, the solid product was separated by filtration, washed with isopropanol and air-dried to obtain a magnetic nanoparticle-modified water-absorbing resin for later use.
[0058] (3) 20% by weight of the nanoparticle-modified water-absorbent resin described in this embodiment is added to 42.5% ordinary silica cement, and then clean water is added according to a water-cement ratio of 0.5, and stirred at a speed of 100 rpm for 5 min. The obtained slurry is poured into a mold and naturally cured for 24 h. After demolding, it is placed in a standard curing room and continued to be cured until the 28th day, thereby obtaining a porous cement-based material.
[0059] The reflectivity was measured by sweeping the frequency using the bow method, and the test frequency range was between 2GHz and 18GHz. At a wave frequency of 2.56 GHz, the reflectivity of the porous cement-based material of this embodiment to electromagnetic waves was -9.67dB. At a wave frequency of 17.28 GHz, the reflectivity of the porous cement-based material to electromagnetic waves was -5.12dB. Using an infrared thermal imager, it was measured that the temperature change of the porous cement-based material of this embodiment within 1 hour after absorbing electromagnetic waves was 12.6°C. Using a universal testing machine, it was measured that the 28d compressive strength of the porous cement-based material of this embodiment was 24.6MPa.
[0060] Example 6 A preparation process of an electromagnetic shielding porous cement-based material comprises the following steps: (1) Magnetic nanoparticles (nano nickel powder with a particle size of 20-90 nm) were vacuum dried and activated at 80°C for 2 h, then added to a dispersion medium (n-heptane) and ultrasonicated for 40 min, then a surfactant (Span 60) was added and heated to 80°C and stirred at this temperature for 10 min to obtain a dispersion for use. The mass ratio of the magnetic nanoparticles, surfactant, and dispersion medium was 1:0.3:6.
[0061] (2) A commercially available water-absorbing resin (model JB40-80, Renqiu Quanxing Chemical Co., Ltd.) was added to water and soaked for 12 hours, with a mass ratio of 1.5:5. The obtained gel material was then added to the dispersion (volume ratio of 1:8) and stirred for 3 hours. After completion, the solid product was separated by filtration, washed with anhydrous ethanol and dried to obtain a magnetic nanoparticle-modified water-absorbing resin for later use.
[0062] (6) Add 5% by weight of the magnetic nanoparticle-modified water-absorbing resin into 42.5% ordinary silica cement, then add clean water at a water-cement ratio of 0.35 and stir at 200 rpm for 3 min. Pour the obtained slurry into a mold and cure it naturally for 24 h. After demolding, place it in a standard curing room and continue curing until the 28th day to obtain a porous cement-based material.
[0063] The reflectivity was measured by sweeping the frequency using the bow method, and the test frequency range was between 2GHz and 18GHz. At a wave frequency of 2.56 GHz, the reflectivity of the porous cement-based material of this embodiment to electromagnetic waves was -5.4dB. At a wave frequency of 17.28GHz, the reflectivity of the porous cement-based material to electromagnetic waves was -1.7dB. Using an infrared thermal imager, it was measured that the temperature change of the porous cement-based material of this embodiment within 1 hour after absorbing electromagnetic waves was 18.5°C. Using a universal testing machine, it was measured that the 28d compressive strength of the porous cement-based material of this embodiment was 29.3MPa.
[0064] Example 7 A preparation process of a porous cement-based material compatible with electromagnetic shielding and infrared protection, comprising the following steps: (1) The spherical highly absorbent organic polymer (the same as in Example 2) is directly added to the dispersion (the same as in Example 2) and stirred for reaction for 1 hour, wherein the mass ratio of the spherical highly absorbent organic polymer to the dispersion is 1:3. After completion, the solid product is separated by filtration, washed with isopropanol and then air-dried to obtain a core-shell magnetic nanoparticle-modified spherical highly absorbent organic polymer for standby use.
[0065] (2) 20% by weight of the magnetic nanoparticle-modified spherical highly absorbent organic polymer is added to 42.5% ordinary silica cement, and then clean water is added according to a water-cement ratio of 0.5, followed by stirring at a speed of 100 rpm for 5 minutes. The obtained slurry is poured into a mold and naturally cured for 24 hours. After demolding, it is placed in a standard curing room and continues to be cured until the 28th day, thereby obtaining a porous cement-based material.
[0066] The reflectivity was measured by sweeping the frequency using the bow method, and the test frequency range was between 2GHz and 18GHz. At a wave frequency of 2.56 GHz, the reflectivity of the porous cement-based material of this embodiment to electromagnetic waves was -7.72dB. At a wave frequency of 17.28 GHz, the reflectivity of the porous cement-based material to electromagnetic waves was -3.48dB. Using an infrared thermal imager, it was measured that the temperature change of the porous cement-based material of this embodiment within 1 hour after absorbing electromagnetic waves was 1.9°C. Using a universal testing machine, it was measured that the 28d compressive strength of the porous cement-based material of this embodiment was 45.6MPa.
[0067] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A process for preparing a porous cement-based material with electromagnetic shielding compatibility and infrared protection, characterized in that: The steps include: (1) The dispersion medium and the surfactant are mixed, heated and stirred to obtain an oil phase for later use; (2) Add the hydrophilic polymer monomer to water and stir until fully dissolved, then add the initiator and the cross-linking agent, stir evenly to obtain an aqueous phase; (3) adding the aqueous phase to the oil phase and stirring until dispersed, and then carrying out a polymerization reaction under heating and stirring conditions, separating the solid product after completion, washing to obtain a spherical highly water-absorbent organic polymer for later use; (4) adding the spherical highly water-absorbent organic polymer to a liquid phase for soaking, then adding the obtained gel material to a magnetic nanoparticle dispersion medium containing a surfactant, stirring the reaction, separating the solid product, and washing the solid product to obtain a spherical core-shell structured magnetic nanoparticle-modified highly water-absorbent organic polymer; (5) The highly water-absorbent organic polymer is added to cement-based materials to prepare a slurry and then cured to obtain a porous cement-based material.
2. The process for preparing the porous cement-based material with electromagnetic shielding compatibility and infrared protection according to claim 1, characterized in that: In step (1), the mass ratio of the dispersion medium to the surfactant is 1-5:0.025-0.075; Optionally, in step (1), the dispersion medium includes at least one of n-heptane, isooctane, cyclohexane, n-hexane, isobutane, methane, and n-butane; Optionally, in step (1), the surfactant includes at least one of silicone oil, sodium dodecyl sulfate, sodium octadecyl sulfate, Span 60, Span 80, Tween 20, Tween 60, and Tween 80; Optionally, in step (1), the heating temperature is 30-60° C., and the stirring time is 10-30 min.
3. The process for preparing the porous cement-based material with electromagnetic shielding compatibility and infrared protection according to claim 1, characterized in that: In step (2), the mass ratio of the hydrophilic polymer monomer to water is 0.5-1:15-40; Optionally, in step (2), the hydrophilic polymer monomer includes at least one of acrylic acid, methacrylic acid, acrylamide, 2-acrylamide-2-methylpropane sulfonic acid, and sodium vinyl sulfonate.
4. The process for preparing the porous cement-based material with electromagnetic shielding compatibility and infrared protection according to claim 1, characterized in that: In step (2), the mass ratio of the hydrophilic polymer monomer, the initiator, and the cross-linking agent is 0.5-1: 0.025-0.075: 0.005-0.01; Optionally, in step (2), the initiator includes at least one of potassium persulfate, sodium persulfate, ammonium persulfate, hydrogen peroxide, tert-butyl hydroperoxide, tert-butyl peroxy-2-ethylhexanoate, and azobisisobutyronitrile; Optionally, in step (2), the crosslinking agent includes at least one of vinylmethyloxyvinylsilane, divinylbenzene, vinyl acrylic acid, N,N'-methylenebisacrylamide, and methyl trimethacrylate; Optionally, in step (2), the stirring time is 10 to 30 minutes.
5. The process for preparing the porous cement-based material with electromagnetic shielding compatibility and infrared protection according to claim 1, characterized in that: In step (3), the mass ratio of the water phase to the oil phase is 2:8; optionally, the water phase is added to the oil phase and stirred for 10 to 30 minutes.
6. The process for preparing the porous cement-based material with electromagnetic shielding compatibility and infrared protection according to claim 1, characterized in that: In step (3), the heating temperature is 50-100° C. and the stirring time is 1-3 h; Optionally, in step (3), the solid product is washed with any one of anhydrous ethanol, isopropanol, dichloromethane and ether.
7. The process for preparing the porous cement-based material with electromagnetic shielding compatibility and infrared protection according to claim 1, characterized in that: In step (4), the mass ratio of the spherical highly absorbent organic polymer to the liquid phase is 0.5-1.1:1-5; Optionally, in step (4), the liquid phase includes any one of aqueous ammonia, white vinegar solution, and water; Optionally, in step (4), the mass fraction of the ammonia water and white vinegar solution is 10-30%; Optionally, in step (4), the soaking time is 12 to 24 hours.
8. The process for preparing the porous cement-based material with electromagnetic shielding compatibility and infrared protection according to claim 1, characterized in that: In step (4), the volume ratio of the gel substance to the magnetic nanoparticle dispersion containing a surfactant is 1:3-8; the mass ratio of the magnetic nanoparticles, the surfactant, and the dispersion medium is 1:0.05-0.3:2-6; Optionally, in step (4), the dispersion medium includes at least one of n-heptane, isooctane, cyclohexane, n-hexane, isobutane, methane, and n-butane; Optionally, in step (4), the surfactant includes at least one of silicone oil, sodium dodecyl sulfate, sodium octadecyl sulfate, Span 60, Span 80, Tween 20, Tween 60, and Tween 80.
9. The process for preparing the porous cement-based material with electromagnetic shielding compatibility and infrared protection according to claim 1, characterized in that: The magnetic nanoparticle dispersion containing a surfactant is prepared by the following method: the magnetic nanoparticles are first vacuum dried and activated for 2-8 hours, and then dispersed in the dispersion medium for ultrasonic treatment for 10-40 minutes; after completion, the surfactant is added, and then heated to 50-80° C. and stirred for 10-30 minutes; Optionally, in step (4), the magnetic nanoparticles include at least one of nano-Fe3O4, nano-cobalt powder, and nano-nickel powder; Optionally, in step (4), the particle size of the magnetic nanoparticles is 20-90 nm; Optionally, in step (4), the stirring reaction time is 1 to 3 hours; Optionally, in step (4), the solid product is washed with any one of anhydrous ethanol, isopropanol, dichloromethane and ether.
10. The process for preparing the porous cement-based material with electromagnetic shielding compatibility and infrared protection according to any one of claims 1 to 9, characterized in that: In step (5), the magnetic nanoparticle-modified spherical highly absorbent organic polymer accounts for 5-20% of the mass of the cement-based material.
Citation Information
Patent Citations
Preparation method of concrete inner curing agent with core-shell structure
CN104788605A
3D printing electromagnetic wave-absorbing concrete with air holes
CN116496045A
Modified super absorbent resin suitable for alkali-activated foam concrete and preparation process of modified super absorbent resin
CN117402293A
Water absorbent containing temperature-sensitive, water-absorbing and-releasing resin, and method for decreasing water content of powdered or particulate material using water absorbent
JP1993179148A
Method for producing granulated material
US6210625B1
Cited By
Cement-based wave-absorbing material and preparation method thereof
CN120622862A