Method for preparing cristobalite micro-nanofiber aerogel based on potassium hexatitanate induction
Preparation of quartzite micro-nanofiber aerogel through potassium hexititate induced, solving the mechanical properties of high-temperature heat-resistant aerogels at extreme temperatures, and achieving high-temperature stability and mechanical properties of materials. It is suitable for High temperature application scenarios.
Patent Information
- Application Number
- CN202411147940.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing high-temperature heat-resistant aerogels have problems with mechanical properties, thermal shrinkage and brittleness at extreme temperatures. The preparation process is complex and costly, making it difficult to meet the needs of high-temperature applications.
The preparation of cune stone micro-nanofiber aerogel by potassium hexititate induction, and the precursor of micro-nanofiber aerogel was prepared by centrifugal spinning, and the nanofiber aerogel was sintered at high temperature to form nanofiber aerogel, and the PTW powder doped with SiO2 to form crystals SiO2 fiber improves the high temperature stability and mechanical properties of the material.
It has achieved improvements in the structural stability and mechanical properties of materials at high temperatures, reduced production costs, and better thermal insulation and mechanical properties. It is suitable for high-temperature environments such as high-speed aviation and commercial spacecraft.
Smart Images

Figure CN119038973A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of nanofiber aerogels, and in particular to a method for preparing cristobalite micro-nano fiber aerogels based on potassium hexatitanate induction. Background Art
[0002] High temperature resistant thermal insulation aerogels are widely used in many fields due to their excellent thermal insulation performance and light weight and high strength. However, current materials also have some shortcomings and disadvantages in practical applications, such as manufacturing cost and complexity. The preparation process of high temperature resistant thermal insulation aerogels usually involves complex chemical reactions and high energy consumption drying processes (such as supercritical drying), which not only significantly increases the production cost, but also limits large-scale production. Although high temperature resistant thermal insulation aerogels are designed to withstand high temperatures, at extreme temperatures, most materials will experience a decrease in mechanical properties or thermal shrinkage leading to structural collapse and loss of mechanical properties, making it difficult to meet the requirements of use. In addition, although some high temperature resistant thermal insulation aerogels show good mechanical strength, many aerogel materials still show significant brittleness and severe pulverization, which limits their application in certain scenarios, especially in situations where the material needs to have a certain degree of flexibility or impact resistance.
[0003] As a SiO2 crystal formed under extremely high temperatures, cristobalite exhibits excellent high-temperature stability. The rapid temperature changes during natural volcanic eruptions and the special conditions in volcanic ash are key factors in promoting the transformation of amorphous SiO2 to a crystalline state (such as cristobalite). This process may involve two main mechanisms: first, the minerals or chemicals that may exist in the volcanic ash act as crystal nuclei to promote crystal growth; second, rapid quenching helps lock the crystal structure and prevent it from degrading during the cooling process. These processes in nature are of great significance for a deep understanding of the preparation conditions of cristobalite and the crystallization process of SiO2, and have potential application value in the fields of fireproof and high-temperature resistant materials and advanced ceramics. At present, there has been no report on the application of cristobalite as micro-nano fiber aerogel insulation material, which deserves in-depth research. Summary of the invention
[0004] In order to solve the technical problems existing in the high temperature resistant thermal insulation aerogel in the prior art, the present invention proposes a method for preparing cristobalite micro-nano fiber aerogel based on potassium hexatitanate induction and a preparation method thereof. Converting cristobalite into micro-nano fiber aerogel material can not only make full use of its stability at high temperatures, but also greatly improve the thermal insulation effect through the high specific surface area and porosity unique to micro-nano fibers. The introduction of micro-nano fiber structure also brings better mechanical properties, which is crucial for protecting the integrity and application life of the material under extreme conditions. Cristobalite thermal insulation materials in the form of micro-nano fibers are expected to play a key role in high-speed aviation, commercial aerospace vehicles and other high-temperature operating environments due to their unique microstructure and physicochemical properties, such as thermal stability and mechanical strength, and meet the requirements for high-performance materials in these fields.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is:
[0006] The first aspect of the present invention provides a method for preparing cristobalite micro-nano fiber aerogel based on potassium hexatitanate induction, comprising the following steps:
[0007] (1) adding PTW powder to a polyvinyl pyrrolidone aqueous solution, stirring, then adding phosphoric acid to adjust the pH, and after adjusting the pH, adding tetraethyl silicate, stirring, and then obtaining a spinning solution;
[0008] (2) The spinning solution is centrifugally spun to obtain a micro-nano fiber aerogel precursor, and then the micro-nano fiber aerogel precursor is placed in a muffle furnace for high-temperature sintering to obtain the cristobalite micro-nano fiber aerogel.
[0009] Preferably, in step (1), the concentration of the polyvinyl pyrrolidone aqueous solution is 14-16 wt %; in some preferred embodiments of the present invention, the concentration of the polyvinyl pyrrolidone aqueous solution is 15 wt %.
[0010] Preferably, in step (1), the mass ratio of the PTW powder to the polyvinyl pyrrolidone aqueous solution is (0.005-0.04):1; further preferably, the mass ratio of the PTW powder to the polyvinyl pyrrolidone aqueous solution is (0.008-0.012):1; further preferably, the mass ratio of the PTW powder to the polyvinyl pyrrolidone aqueous solution is 0.01:1.
[0011] Preferably, in step (1), the pH value after adding the phosphoric acid to adjust the pH is 4-5.
[0012] Preferably, in step (1), the mass ratio of the tetraethyl silicate to the polyvinyl pyrrolidone aqueous solution is (0.2-0.4):1.
[0013] Preferably, in step (2), when the spinning solution is subjected to centrifugal spinning, an airflow-assisted centrifugal spinning device is used.
[0014] Further preferably, the structure of the airflow-assisted centrifugal spinning device includes: a fan, a motor, a liquid storage tank, and a conveyor belt designed from top to bottom.
[0015] The main structure of the airflow-assisted centrifugal spinning device of the present invention includes a fan, a motor, a liquid storage tank and a conveyor belt for collection. After the needle and the liquid storage tank are installed, the prepared polymer solution is loaded into the nozzle or the injector to start the device, so that the nozzle starts to rotate, the liquid storage tank rotates at high speed driven by the motor, and the solution is sprayed out through the rotating nozzle, and then stretched into filaments under the action of centrifugal force, while the solvent evaporates, and finally forms fibers, which are deposited on the conveyor belt under the wind force of the fan above the device to obtain the precursor of micro-nano fiber aerogel.
[0016] Further preferably, the airflow-assisted centrifugal spinning device uses a 27G needle and the motor speed is 4000-6000r / min.
[0017] Preferably, in step (2), the high temperature sintering parameters are: heating to 1000-1300° C. at a heating rate of 4-6° C. / min and then taking out.
[0018] The second aspect of the present invention provides a cristobalite micro-nano fiber aerogel, which is prepared by the method for preparing cristobalite micro-nano fiber aerogel based on potassium hexatitanate induction.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] The present invention prepares a micro-nano fiber aerogel precursor based on a centrifugal spinning method, and sintering it into a nanofiber aerogel at a high temperature. By doping PTW in the raw material to induce SiO2 nanofibers to form crystalline SiO2 fibers, a high-temperature resistant quartz nanofiber aerogel material is finally obtained. The high efficiency and low cost of the centrifugal spinning method give it the potential for large-scale and batch production. In addition, the micro-nano fiber aerogel material can provide better structural stability due to the cross-linked network between its fibers, so that it maintains low thermal conductivity while having good mechanical properties, which is more advantageous in some applications that require both thermal insulation and mechanical properties. In addition, by inducing SiO2 micro-nano fiber aerogel to form quartz micro-nano fiber aerogel, the advantages of crystalline SiO2 and fiber aerogel are combined, breaking through the problem of SiO2 micro-nano fiber aerogel collapsing above 1300°C and deteriorating mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 Schematic diagram of the preparation process of nanofiber aerogel;
[0022] Figure 2 It is a schematic diagram of a centrifugal spinning device;
[0023] Figure 3 The XRD test results of samples 1-5 and the standard card spectra of SiO2, TiO2 and K2O·6TiO2;
[0024] Figure 4 IR spectra of sample No. 3 and pure SiO2 and TiO2 samples;
[0025] Figure 5 The SEM image and internal element distribution diagram of sample 3;
[0026] Figure 6 This is the graph of thermal conductivity of sample No. 3 changing with temperature;
[0027] Figure 7 SEM images of samples A and B;
[0028] Figure 8 is the EDS diagram of sample A and B;
[0029] Fig. 9 The distribution diagram of elements inside the fiber of samples A and B;
[0030] Fig.10 The stress-strain curves of samples A and B. The insets are pictures of different states during the compression process: original state - compression 50% - return to the original state. DETAILED DESCRIPTION
[0031] The specific embodiments of the present invention are further described below. It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention. In addition, the technical features involved in each embodiment of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0032] The experimental methods in the following examples are conventional methods unless otherwise specified, and the experimental materials used in the following examples are commercially available unless otherwise specified.
[0033] Example 1
[0034] (1) Preparation of spinning solution: PTW powder (K2O·6TiO2) was milled in a planetary ball mill at a speed of 400 r / min, in a forward direction for 30 min and a reverse direction for 30 min for 10 h to obtain PTW fine powder with a particle diameter of less than 1 μm, which was stored for later use. Polyvinyl pyrrolidone (PVP) particles were added to pure water and stirred continuously at a speed of 500 r / min using a mechanical stirrer until completely dissolved to obtain a basic solution: a 15 wt% PVP aqueous solution. Take 5 parts of the same mass of basic solution, numbered 1, 2, 3, 4, and 5, and then add PTW fine powder to the basic solution at a ratio of 0g, 0.05g, 0.1g, 0.2g, and 0.4g of PTW per 10g of basic solution, stirring and adding, stirring for 10min after the addition is completed, add phosphoric acid (PA) to the solution at a ratio of 0.02g per 10g of basic solution with a pipette, stirring and adding, after adding, dip a drop of solution with a glass rod every 2min to test the pH of the solution with pH test paper, if the pH of the solution is higher than 5, continue to add PA as needed, test every 2min until the pH is between 4 and 5. After adjusting the pH, continue to add tetraethyl silicate (TEOS) to the basic solution at a ratio of 3g per 10g of basic solution, stirring and adding, stirring for 120min after the addition is completed, and the spinning solution is ready. The specific ratio is shown in Table 1.
[0035] Table 1 Doping amount of K2O·6TiO2
[0036]
[0037] (2) Centrifugal spinning: After the spinning solution is prepared, spinning should be done immediately. During the stirring of the solution, the centrifugal spinning equipment can be prepared. The present invention uses a self-built spinning equipment, such as Figure 2 As shown, the whole device consists of a fan, a motor, a liquid storage tank and a conveyor belt for collection. After the needle and the liquid storage tank are installed, the prepared polymer solution is loaded into the nozzle or injector to start the equipment and make the nozzle start to rotate. The liquid storage tank rotates at high speed driven by the motor, and the solution is sprayed out through the rotating nozzle, and then stretched into filaments under the action of centrifugal force. At the same time, the solvent evaporates and finally forms fibers. Finally, under the action of the wind force of the fan above, it is deposited on the conveyor belt to obtain the precursor of micro-nano fiber aerogel. A 27G needle is selected, and the motor speed is 5000r / min.
[0038] (3) Post-treatment: The micro-nano fiber aerogel collected during the spinning process is simply trimmed and placed in a muffle furnace. After heating to 1000°C at a heating rate of 5°C / min, it is kept warm for 2 hours, taken out, and cooled at room temperature to obtain the desired micro-nano fiber aerogel.
[0039] The XRD spectra of samples 1-5 and standard cards of cristobalite, PTW and titanium dioxide are shown in the attached Figure 3 As shown, the half-peak widths of samples 1-5 were obtained by iterative fitting through the Gaussian function of the Origin drawing software, which were 13.0°, 8.5°, 0.9°, 1.1°, and 1.0°, respectively. Sample 3 had the narrowest half-peak width, indicating that its internal grains were relatively large and the lattice defects were minimal. Figure 3 , sample 1 (undoped with PTW) exhibits the characteristics of amorphous SiO2 micro-nanofiber aerogel, i.e., there is no obvious crystal peak, showing a flat baseline, which indicates that without the addition of PTW, amorphous SiO2 does not transform into any crystalline form at this temperature. In contrast, the XRD spectra of samples 2, 3, 4 and 5 doped with different amounts of PTW show obvious diffraction peaks, which match the peaks on the standard XRD cards of cristobalite. Compared with the standard cards of PTW and titanium dioxide, it can be seen that PTW has been decomposed during the sintering process, but it is still difficult to exclude the presence of titanium dioxide. Generally, the conversion of SiO2 from amorphous to crystalline requires higher energy than the conversion between crystalline states, which is sufficient to prove that the doping of PTW can reduce the crystallization temperature of amorphous SiO2 and successfully induce the conversion of amorphous SiO2 into crystalline cristobalite. Moreover, it can be seen from the spectrum that with the increase of PTW doping amount, from sample No. 1 to sample No. 3, the diffraction peaks in the XRD spectrum become more intense and the half-peak width becomes narrower, which means that the crystal particles become larger and the content increases. However, in samples 4 and 5, even when the amount of PTW increased to 0.4 g, the peak intensity did not continue to increase significantly, but was lower than before, and the half-peak width was also increasing. This shows that after a certain doping amount, further increasing PTW does not lead to the formation of more crystalline SiO2, which may mean that after the amount of dopant exceeds a certain threshold, the crystallization process of SiO2 no longer increases the number of crystals or grain size.
[0040] The IR spectra of sample No. 3 and nano-titanium dioxide (TiO2) and SiO2 powders are as follows: Figure 4 As shown, for SiO2, the typical absorption peak appears at about 1100 cm -1 This is related to the vibration frequency of the Si-O-Si bond. If there is significant titanium dioxide (TiO2) in the sample, you would typically expect a band around 400-800 cm -1 The characteristic peaks can be seen in the area. From the figure, we can see that the main absorption peaks of the samples are concentrated at 1100cm -1 This indicates that the sample is mainly composed of SiO2. In addition, there is a lack of -1The obvious absorption peak in the region indicates that titanium dioxide does not exist in the sample, or its content is so low that it cannot be detected in the IR spectrum. Combining this information, it can be reasonably inferred that sample 3 is crystalline or amorphous SiO2, and the doping process does not introduce titanium dioxide, or its content is very low.
[0041] The SEM image and internal element distribution of sample 3 are shown in Figure 5 As shown in the figure, the first figure is the SEM image of the fiber. It can be seen from the figure that the diameter of the fiber is about 1μm, which is consistent with the typical results of centrifugal spinning technology. Although centrifugal spinning technology has the ability to prepare nano-scale fibers, in practice, the diameter of the fiber is often in the micron level, which is related to a variety of parameters, including polymer concentration, solution viscosity and surface tension, solution evaporation rate, spinning equipment rotation speed, needle diameter, fiber collection distance, ambient humidity and temperature, etc. The SEM image also shows that most of the fiber surfaces are smooth. The smoothness of the fiber surface indicates good continuity and uniformity, which is beneficial for enhancing the mechanical properties and functionalization of the material. However, protrusions can still be seen on the surface of a few fibers, which may be due to the excessive growth of quartz grains in some fibers. This excessive growth of grains may be due to local component oversaturation or uneven conditions during heat treatment. The remaining pictures are EDS element distribution diagrams, from which we can see that silicon (Si) and oxygen (O) elements are evenly distributed throughout the sample, and the distribution of potassium (K) also shows high uniformity, which indicates that PTW is decomposed during the preparation process, and its potassium ions are released and evenly distributed in the fiber, while titanium atoms are not. It can be inferred that potassium ions may have played a role in inducing crystal growth, while titanium atoms may not be dispersed due to certain conditions during the crystal growth process, such as temperature, solvent environment, or the kinetics of other chemical reactions.
[0042] The thermal conductivity of sample 3 is Figure 6 As shown in the figure, the thermal conductivity at room temperature is only 0.0411W / (m·K). When the temperature rises to 800℃, the thermal conductivity is only 0.1004W / (m·K). The thermal insulation performance is still excellent and can meet the application needs in most cases.
[0043] High temperature resistance test: Trim sample 3 into a suitable shape and put it into a corundum boat, then put the corundum boat into the middle of the corundum tube of the tubular furnace, and plug the two sides with pipe plugs to reduce energy loss. Then seal the tube cover and open the valves at both ends to keep the pressure inside and outside the corundum tube balanced during heating. Then set the same heating rate, that is, 5℃ / min, heat to the corresponding required temperature and keep the heating rate for three hours, and then take out the sample after natural cooling in the furnace. Since the melting point of PTW is 1370℃, 1300℃ and 1400℃ are set to preliminarily explore the heat resistance limit range of quartz micro-nano fiber aerogel induced by PTW, as well as the morphology and performance changes of the material before and after heating. This group of experimental conditions and experimental phenomena are shown in Table 2:
[0044] Table 2 High temperature test conditions and phenomena
[0045] Experiment number Experimental conditions Experimental phenomenon First No heating No change Second Heat to 1300℃ at 5℃ / min, keep warm for 3h There is little change in the macro sense, only some contraction C Heat to 1400℃ at 5℃ / min, keep warm for 3h Most of the fibers melted, and the remaining part was severely powdered.
[0046] After sample B was heated and kept at 1300℃ for 3 hours, the sample did not change much macroscopically, with only some shrinkage. This shows that the quartz nanofiber-based material has a certain heat resistance at this temperature and a relatively stable structure. The shrinkage phenomenon may be due to the evaporation of moisture or other volatile components inside the material due to high-temperature treatment, as well as the cooling shrinkage after thermal expansion; after sample C was heated and kept at 1400℃ for 3 hours, most of the fibers melted and the remaining part was severely powdered. This shows that the quartz nanofiber-based material exceeded its heat resistance limit at this temperature and its structural integrity was seriously damaged. Although PTW has long been decomposed in a sintering environment of 1000℃, its decomposed components may still promote the melting process at 1400℃, resulting in large-scale structural damage to the material.
[0047] The SEM images of samples A and B are shown in Figure 7As shown in the figure, it can be seen from the SEM image that the fiber surface of sample A is relatively smooth, which may be due to the shortage of sintering time or the temperature not reaching the optimal conditions for grain growth, so that the grains do not have enough time to grow to a larger size, resulting in the formation of uniform and finer grains uniformly wrapped in the fiber. A small number of fiber surfaces have protrusions, which may be due to the local temperature being too high or the uneven distribution of doping substances causing the grains to grow too large. Relatively speaking, the fiber surface of sample B showed significant protrusions at a high temperature of 1300℃ and after 3 hours of heat preservation, which indicates that the grains have sufficient time to grow under the conditions of higher temperature and longer time, resulting in the formation of larger grains. In addition, there are many more holes on the fiber surface of sample B, which may be due to the fact that the potassium ions doped in the sample are converted into potassium oxide at high temperature, and flow out or volatilize during liquefaction or gasification, leaving holes. Since the melting point of potassium oxide is about 740℃, it is easy to lose or volatilize after liquefaction. The titanium atoms may be transformed into titanium dioxide with a higher melting point (melting point is about 1843°C), which is still stable at the highest temperature of the experiment, so they remain in the fibers and may participate in or affect the growth process of the grains. This change in microstructure has a direct impact on the macroscopic properties of the material. The appearance of pores may affect the mechanical strength and thermal stability of the material, but it may also increase the specific surface area of the material, which may be beneficial in some applications. For example, in catalytic or filtration applications, a larger specific surface area can provide more active sites or filtration paths.
[0048] The EDS images of samples A and B are shown in Figure 8 As shown, Figure a is the EDS graph of sample A, and Figure b is the EDS graph of sample B, showing the X-ray emission peaks of different elements in the sample. These peaks correspond to the specific energies of the elements in the sample and can be used to determine the elemental composition of the sample. The peaks in the figure are marked to indicate the elements they represent, such as O for oxygen, Si for silicon, Al for aluminum, C for carbon, Pt for platinum, K for potassium, and Ti for titanium. Among them, Al is an aluminum electron microscope stage, and C and Pt are conductive coatings used in the sample preparation process. This is a standard sample preparation step designed to reduce charge accumulation, so they need to be excluded during analysis. Although phosphoric acid is added to the raw material, there is no phosphorus (P) in the spectrum. It may be that phosphoric acid (boiling point is about 158°C) is evaporated during the heating process. Even if the small amount left behind forms phosphates or oxides, due to the relatively low thermal stability of phosphates at high temperatures, when the temperature rises, they will eventually become phosphorus pentoxide (P2O5) and sublime. Figure 8 In a, silicon (Si) and oxygen (O) are the main elements, and their high peaks indicate that they are the main components of the sample. The characteristic peaks of potassium (K) and titanium (Ti) indicate the doping of PTW. Figure 8b, note that the characteristic peak of potassium (K) disappears, indicating that after a higher temperature sintering process, the potassium component has volatilized or dissociated from the sample. At the same time, the peak of titanium (Ti) still exists, and its content is relatively stable compared with sample A, which indicates that the titanium element remains stably in the sample during the sintering process, proving that potassium ions are lost during further high-temperature sintering, while titanium atoms are retained.
[0049] Figure 8 a and Figure 8 The right side of b also provides the elemental composition information normalized by mass percentage (Mass%) and atomic percentage (Atom%). By comparing the titanium content in the two spectra, it can be seen that the titanium content is basically relatively consistent in the two samples, which indicates that although sample A and sample B are processed under different sintering conditions, the doped PTW may be distributed fairly evenly in the material.
[0050] The distribution diagram of the elements inside the fiber of samples A and B is shown in Fig. 9 As shown, Fig. 9 a corresponds to sample A, Fig. 9 b corresponds to sample B. Fig. 9 In sample b, silicon (Si) is still widely distributed, but potassium (K) is gone. However, titanium (Ti) is still distributed in clusters, which indicates that even after sintering at a higher temperature, titanium still exists in the fiber in a stable aggregated state, without significant diffusion or distribution changes. Sample B at 1300°C does not contain potassium (K), and its structure is still intact. This indirectly proves that the melting of sample C at 1400°C is not caused by potassium ions, but may be the influence of titanium (Ti). Because the melting point of pure cristobalite is around 1610°C, it will not fail thermally at 1400°C.
[0051] A universal testing machine was used to perform a compression test on the material. The required samples were cut into a size of 2cm*2cm*1cm. The densities of samples A and B are shown in Table 3 below.
[0052] Table 3
[0053] Sample name Length(cm) Length(cm) Length(cm) Mass (mg) <![CDATA[Density (mg / cm 3 )]]> First 2 2 1 71.7 17.9 Second 2 2 1 82.9 20.7
[0054] By calculation, we can know that the density of sample A at 1000℃ is 17.9mg / cm 3 , while the density of sample B heated to 1300℃ is slightly higher, which is 20.7mg / cm 3 It should be that further high temperature and heat preservation promote the crystallization of the amorphous region. Due to the reorganization of the internal molecular structure during crystallization, from disorder to order, the volume is reduced. The overall reduction is reflected in the macroscopic state, and the mass is not lost in this process, so the density increases.
[0055] The compression test of the material was completed by a universal testing machine. Samples A and B were compressed to 50% respectively. After 20 cycles of compression, the average value of the obtained data was taken and then plotted using a drawing software. See Fig.10 .from Fig.10 It can be clearly observed that with the increase of compression strain, the stress increases faster and faster. This is because as the machine is compressed, the density of the material is gradually increasing, and it is increasing nonlinearly. Moreover, under the same strain, the stress of material B is significantly higher than that of material A. This is because high-temperature sintering makes material B more crystallized, and crystallized materials are often harder and more difficult to deform. Moreover, the density is higher, and there are more stressed fibers under the same volume, which is manifested as higher stress under the same deformation on the stress-strain curve. According to the rebound curve, even after being calcined at a high temperature of 1300°C for 3 hours, the fiber aerogel still maintains excellent mechanical properties, which also shows that the aerogel not only has no thermal failure, but has better performance.
[0056] The present invention uses PTW as a dopant to induce amorphous SiO2 to crystallize into cristobalite at a relatively low temperature. The success of this research lies in the discovery of an effective way to achieve high-temperature phase SiO2 crystallization at a lower temperature, while also solving the problem of structural collapse and thermal failure of SiO2 fibers at 1300°C.
[0057] Micro-nano fibers were prepared by centrifugal spinning technology, and the materials were characterized by XRD, IR, SEM, EDS and other techniques. The experimental results show that with the increase of PTW doping amount, the crystallinity of the aerogel increases, showing a narrower half-peak width. In addition, the high temperature treatment (1000℃ to 1400℃) experiment revealed the heat resistance and structural stability of the material, especially at 1300℃, the material showed good heat resistance, mechanical properties and structural integrity. The development of this material has important practical application value for high temperature application scenarios, such as refractory materials, high temperature filters and catalyst carriers.
[0058] The present invention not only confirms the feasibility of using PTW to induce amorphous SiO2 to crystallize into cristobalite, but also successfully controls the crystallization process and microstructure by adjusting the doping amount, thereby optimizing the performance of the material. In addition, the performance of the material under high temperature conditions indicates that it has broad application prospects in high temperature application fields such as aerospace, energy and electronics industries.
[0059] The embodiments of the present invention are described in detail above, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations of these embodiments are made without departing from the principles and spirit of the present invention, and still fall within the protection scope of the present invention.
Claims
1. A method for preparing cristobalite micro-nano fiber aerogel based on potassium hexatitanate induction, characterized in that: The following steps are involved: (1) adding PTW powder to a polyvinyl pyrrolidone aqueous solution, stirring, then adding phosphoric acid to adjust the pH, and after adjusting the pH, adding tetraethyl silicate, stirring, and then obtaining a spinning solution; (2) The spinning solution is centrifugally spun to obtain a micro-nano fiber aerogel precursor, and then the micro-nano fiber aerogel precursor is placed in a muffle furnace for high-temperature sintering to obtain the cristobalite micro-nano fiber aerogel.
2. The method for preparing cristobalite micro-nano fiber aerogel based on potassium hexatitanate induction according to claim 1, characterized in that: In step (1), the concentration of the polyvinyl pyrrolidone aqueous solution is 14-16 wt %.
3. The method for preparing cristobalite micro-nano fiber aerogel based on potassium hexatitanate induction according to claim 1, characterized in that: In step (1), the mass ratio of the PTW powder to the polyvinyl pyrrolidone aqueous solution is (0.005-0.04):
1.
4. The method for preparing cristobalite micro-nano fiber aerogel based on potassium hexatitanate induction according to claim 1, characterized in that: In step (1), the pH value after adding the phosphoric acid to adjust the pH is 4-5.
5. The method for preparing cristobalite micro-nano fiber aerogel based on potassium hexatitanate induction according to claim 1, characterized in that: In step (1), the mass ratio of the tetraethyl silicate to the polyvinyl pyrrolidone aqueous solution is (0.2-0.4):
1.
6. The method for preparing cristobalite micro-nano fiber aerogel based on potassium hexatitanate induction according to claim 1, characterized in that: In step (2), when the spinning solution is subjected to centrifugal spinning, an airflow-assisted centrifugal spinning device is used.
7. The method for preparing cristobalite micro-nano fiber aerogel based on potassium hexatitanate induction according to claim 6, characterized in that: The structure of the airflow-assisted centrifugal spinning device includes: a fan, a motor, a liquid storage tank, and a conveyor belt, which are designed from top to bottom.
8. The method for preparing cristobalite micro-nano fiber aerogel based on potassium hexatitanate induction according to claim 6, characterized in that: The airflow-assisted centrifugal spinning device uses a 27G needle and the motor has a rotation speed of 4000-6000 r / min.
9. The method for preparing cristobalite micro-nano fiber aerogel based on potassium hexatitanate induction according to claim 1, characterized in that: In step (2), the high temperature sintering parameters are: heating to 1000-1300°C at a heating rate of 4-6°C / min and then taking out.
10. A cristobalite micro-nano fiber aerogel, characterized in that: The aerogel is prepared by the method for preparing cristobalite micro-nano fiber aerogel based on potassium hexatitanate induction as described in any one of claims 1 to 9.
Citation Information
Patent Citations
Aramid fiber micro-nano fiber aerogel material and preparation method thereof
CN117684279A
Elastic ceramic micro-nanofiber aerogel thermal insulation material as well as preparation method and application thereof
CN117902884A
Preparation method of cristobalite content controllable photocuring 3D printing silicon-based ceramic core
CN118359425A
Cited By
Method for generating cristobalite aerogel based on induction of potassium phosphate and magnesium phosphate
CN119593109A
Flexible cristobalite fiber aerogel as well as preparation method and application thereof
CN120622913A