Pug for reducing characteristics of Macang soil and process for manufacturing ceramic product of pug
By optimizing the formula and process of clay materials, combining a variety of minerals and additives, the reduction of Makang ceramic products has been achieved, solving the problems of limited resources of Makang soil and irreplaceable firing characteristics, and obtaining Makang soil characteristics Ceramic products.
Patent Information
- Application Number
- CN202411229450.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing technology cannot completely replace Makang soil, and cannot produce ceramic products with Makang soil characteristics. Makang soil resources are limited and the fired porcelain lacks physical and chemical indicators and sensory impressions.
By optimizing the formula and manufacturing process of clay materials, combining the ratios of quartz, sericite, plagioclase, kaolinite, mica, cobalt oxide, polystyrene, iron oxide, potassium oxide, sodium oxide and water, using segmented parts Fired and multiple stale processes to make ceramic products with goose egg cyan, bulb and flint red characteristics.
We successfully obtained ceramic products with the characteristics of Makang soil. The surface is green and there is a bulging phenomenon. There is obvious flint red at the joint between the bottom and the glaze layer. It has excellent performance and meets the research needs of imitating Makang soil ceramic products.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ceramics, and in particular relates to a clay material capable of restoring the properties of Macang clay and a process for manufacturing ceramic products thereof. Background Art
[0002] Macang clay is a kind of kaolin produced in Macang Mountain near Jingdezhen, and is one of the main raw materials for making porcelain. The raw material for making porcelain in Jingdezhen during the Yuan and Ming dynasties was a kind of kaolin produced in Macang Mountain near Jingdezhen, hence the name. Macang clay is one of the main raw materials for making porcelain. It is a rock-like mineral mainly composed of quartz and sericite. The color is white with a slight hint of yellow, green, gray or light red. It has been used to make porcelain in my country for a long time. Macang clay is characterized by being white but not fine, and having many pores. The bottom of porcelain fired with Macang clay has a natural and obvious flint red, with black moles, and the fired porcelain has bulging, or the glaze surface has cracks or brown eyes.
[0003] Due to the limited resources of Macang clay, the clay mining of Macang Mountain was almost exhausted as early as the Jiajing period of the Ming Dynasty. Although kaolin was subsequently used as clay to replace Macang clay, kaolin and Macang clay are not exactly the same. Macang clay has the characteristics of blue-black seams, sugar spots, white jade, and gold star colors. The bottom of the fired porcelain has natural and obvious flint red, and there are also small bulges, or the glaze has cracks or gaps, and some have brown eyes, while porcelain fired with kaolin does not have the above phenomena. In addition, kaolin is white and fine, without pores. After firing, it is dense and has no natural flint red. It cannot completely replace Macang clay to obtain products with the same physical and chemical indicators and sensory impressions.
[0004] Therefore, developing a clay material that can restore the characteristics of Macang clay can provide a certain basis for the research on Macang clay-like ceramic products. Summary of the invention
[0005] The purpose of the present invention is to provide a clay material that restores the characteristics of Macang clay and a process for manufacturing ceramic products thereof. The clay material formula is optimized by mixing and manufacturing the clay material, and the ceramic products obtained have an egg green surface, bulges, and even brown eyes, and there is obvious flint red at the junction of the bottom and the glaze layer, which has the characteristics of Macang clay porcelain.
[0006] To achieve the above-mentioned purpose, the present invention provides a clay material that restores the characteristics of Macakura soil, wherein the clay material comprises the following raw material components in parts by weight: 40-50 parts of quartz, 20-40 parts of sericite, 10-20 parts of plagioclase, 20-25 parts of kaolinite, 20-25 parts of muscovite, 1-2 parts of cobalt oxide, 0.5-1 parts of strontium carbonate, 2-5 parts of polystyrene, 1-2 parts of iron oxide, 2.5-4 parts of potassium oxide, 2.5-4 parts of sodium oxide, and 35-45 parts of water.
[0007] Macang clay is a kind of porcelain clay discovered and used in the early Yuan Dynasty, but it was exhausted in the Ming Dynasty Wanli. Relevant research on porcelain made with Macang clay points out that Macang clay is white but not fine, with many pores. The bottom of porcelain fired with Macang clay has natural and obvious flint red, black moles, and the fired porcelain has bulging, cracks on the glaze, or brown spots. Therefore, the inventor has studied its characteristics and developed the clay material of the present invention that restores the characteristics of Macang clay, wherein the main component of quartz is silicon dioxide, with few impurities and stable chemical properties; sericite is mainly composed of silicon oxygen tetrahedron and aluminum oxygen octahedron, and may also contain a small amount of Fe2O3 and MgO, etc.; plagioclase is an isomorphous series composed of albite (NaAlSi3O, symbol Ab) and calcium feldspar (CaAl2Si2O8, symbol An), and its chemical formula can be expressed as (Ca, Na)Al(Al, Si)Si2O8, and the above components are similar to the main components of porcelain stone; and kaolinite is the main mineral component of kaolin, and its chemical formula is Al2Si2O5(OH)4, and the chemical composition of muscovite is KAl2(AlSi3O 10 )(OH)2, the above two components are similar to the main chemical components of Makura soil. In addition, by adding a small amount of cobalt oxide as a colorant, a certain goose egg blue color is presented in the porcelain; by adding polystyrene, a certain amount of pores are left after firing; by adding sodium carbonate, the gas produced after being decomposed during high-temperature firing makes the glaze bulge or form brown eyes; by adding a small amount of iron oxide again, it prepares for the subsequent formation of flint red.
[0008] Furthermore, in the above technical solution, the particle size of the quartz is 0.5-2 μm; the particle size of the sericite is 0.1-1 μm; and the particle size of the plagioclase is 1.5-3 μm.
[0009] Furthermore, in the above technical solution, the particle size of the kaolinite is 3-5 μm, and the particle size of the muscovite is 2-8 μm. The present invention limits the particle size of each raw material, thereby eliminating the problem of uncontrollable particle size caused by subsequent mud making and ball milling processes, and the particle size setting has a sense of hierarchy, especially the larger particle sizes of kaolinite and muscovite, which is more in line with the characteristics of Macang soil being white but not fine.
[0010] Furthermore, in the above technical solution, the particle size of the polystyrene is 5-15 μm.
[0011] The present invention also provides a process for manufacturing ceramic products from clay material that restores the properties of Macang clay, comprising the following steps: (1) Prepare all raw materials according to the recipe and set aside; (2) Mix quartz, sericite, plagioclase, kaolinite, muscovite and strontium carbonate evenly, pass through a 500-mesh sieve, add 95% water, and stir evenly; (3) The mixed mud is aged once, and then placed in a vacuum mud kneading machine for mud kneading; (4) Secondary aging of the mixed mud after the first mud kneading; (5) Add the remaining raw materials to the mixed mud after secondary aging, mix well and put it into a vacuum mud kneading machine for secondary mud kneading; (6) Make the clay into a body, dry it, apply a layer of transparent glaze, and let it dry; (7) The dried green body is placed in a kiln and the firing temperature is controlled in stages. After the firing is completed and the green body is cooled, a finished ceramic product is obtained.
[0012] The present invention first mixes quartz, sericite, plagioclase, kaolinite and muscovite into clay and then ages it twice, which can promote the loosening of the clay, improve the performance of the clay, and make the clay more uniform and easy to shape; adding the remaining materials after the second aging can effectively prevent the oxide reaction during the aging process and affect the subsequent firing effect; adopting staged firing, it can be controlled according to the volatilization temperature of the raw materials, and the unique characteristics of Macang clay porcelain can be produced, so as to achieve the purpose of obtaining porcelain with restored Macang clay characteristics.
[0013] Furthermore, in step (3) of the above technical solution, the primary aging process is as follows: the mixed mud is placed in a plastic bag under light-shielded conditions at room temperature for 5-8 days; and the vacuum degree of the mud kneading is >100 kPa.
[0014] Furthermore, in step (4) of the above technical solution, the secondary aging process is: the mixed mud after the first mud kneading is placed in a plastic bag under light-shielded conditions at room temperature for 8-12 days; in step (5), the vacuum degree of the mud kneading is >150 kPa.
[0015] Furthermore, in step (7) of the above technical solution, the process of segmented temperature control is as follows: first heating, raising the temperature to 280-350°C at a rate of 5-8°C / min, and keeping it warm for 2-3h; second heating, raising the temperature to 1600-1700°C at a rate of 4-6°C / min, and keeping it warm for 1-2h; first cooling, lowering the temperature to below 1200°C at a rate of 10-15°C / min; second cooling, natural cooling. In the technical scheme, the polystyrene in the blank is quickly burned out by heating at a relatively fast speed, thereby leaving pores in the blank and improving the air permeability of the blank; then the temperature is raised to above 1600°C, and strontium carbonate with a decomposition temperature slightly lower than the melting temperature of the transparent glaze is used. When the decomposition temperature is reached, the strontium carbonate is decomposed into strontium oxide and carbon dioxide, and the carbon dioxide overflows and breaks through the glaze layer to produce pores. In the process of rapid cooling, the glaze layer is combined, but the strontium carbonate is not completely decomposed and is still at its decomposition temperature, it is easy to form bubbles or brown eyes.
[0016] Furthermore, in the above technical solution, 4-6% of the total volume of flue gas is introduced into carbon monoxide in the secondary heating stage; and 1-2% of the total volume of flue gas is introduced into oxygen in the primary cooling stage. In the technical solution, by introducing appropriate reducing gas in the secondary heating stage, the iron in the body is reduced to ferrous oxide, which is gathered at the bottom of the porcelain or at the junction of the body and glaze. During the cooling process, it is oxidized by a certain amount of oxygen to form red or orange-red flint red.
[0017] The present invention also provides a ceramic with reduced Makura clay properties manufactured by the above process.
[0018] The preparation processes not specifically described in the present invention are all conventional processes.
[0019] The present invention has the following beneficial effects: By optimizing the clay raw material ratio and the manufacturing process, the present invention obtains a ceramic product with excellent performance. The surface is goose egg green with bulges and even brown eyes, and there is obvious flint red at the junction of the bottom and the glaze layer. It has the characteristics of Macang clay porcelain, and provides a certain basis for the research on imitation Macang clay and the manufacture of porcelain. DETAILED DESCRIPTION
[0020] The experimental methods in the following examples are conventional methods unless otherwise specified. The raw materials involved in the following examples are common commercial products and can be purchased from the market unless otherwise specified.
[0021] The present invention is described in further detail below in conjunction with embodiments: Example 1 A process for manufacturing ceramic products from clay material that restores the characteristics of Macang clay, comprising the following steps: (1) Prepare the raw materials according to the formula, including 40 parts of quartz, 20 parts of sericite, 20 parts of plagioclase, 20 parts of kaolinite, 25 parts of muscovite, 1 part of cobalt oxide, 0.8 parts of strontium carbonate, 3 parts of polystyrene, 2 parts of iron oxide, 2.5 parts of potassium oxide, 4 parts of sodium oxide, and 40 parts of water, for later use. The particle size of quartz is 0.5-2 μm; the particle size of sericite is 0.1-1 μm; the particle size of plagioclase is 1.5-3 μm; the particle size of kaolinite is 3-5 μm, the particle size of muscovite is 2-8 μm; and the particle size of polystyrene is 5-15 μm. (2) Mix quartz, sericite, plagioclase, kaolinite, muscovite and strontium carbonate evenly, pass through a 500-mesh sieve, add 95% water, and stir evenly; (3) The mixed mud is placed in a plastic bag and placed at room temperature for 6 days in a dark place for aging, and then placed in a vacuum mud kneading machine with a vacuum degree of >100 kPa for mud kneading; (4) Put the mixed mud after the first mud kneading into a plastic bag and place it at room temperature for 10 days in a dark place for secondary aging; (5) Add the remaining raw materials to the mixed mud after secondary aging, mix well, and put it into a vacuum mud kneading machine with a vacuum degree of >150kPa for secondary mud kneading; (6) Make the clay into a body, dry it, apply a layer of transparent glaze, and let it dry; (7) The air-dried green body is placed in a kiln and fired at a staged temperature control process, wherein the staged temperature control process is as follows: a first heating process, raising the temperature to 300°C at a rate of 5°C / min and keeping the temperature for 2.5 hours; a second heating process, raising the temperature to 1600°C at a rate of 4°C / min, while introducing carbon monoxide in an amount of 4% of the total volume of the flue gas, and keeping the temperature for 1.5 hours; a first cooling process, lowering the temperature to below 1200°C at a rate of 10°C / min and while introducing oxygen in an amount of 1% of the total volume of the flue gas; a second cooling process, natural cooling, and obtaining a finished ceramic product.
[0022] Example 2 A process for manufacturing ceramic products from clay material that restores the characteristics of Macang clay, comprising the following steps: (1) Prepare the raw materials according to the formula, including 45 parts of quartz, 25 parts of sericite, 15 parts of plagioclase, 22 parts of kaolinite, 23 parts of muscovite, 1.5 parts of cobalt oxide, 0.5 parts of strontium carbonate, 5 parts of polystyrene, 1.5 parts of iron oxide, 3 parts of potassium oxide, 3 parts of sodium oxide, and 38 parts of water, for later use. The particle size of quartz is 0.5-2 μm; the particle size of sericite is 0.1-1 μm; the particle size of plagioclase is 1.5-3 μm; the particle size of kaolinite is 3-5 μm, the particle size of muscovite is 2-8 μm; and the particle size of polystyrene is 5-15 μm. (2) Mix quartz, sericite, plagioclase, kaolinite, muscovite and strontium carbonate evenly, pass through a 500-mesh sieve, add 95% water, and stir evenly; (3) The mixed mud is placed in a plastic bag and placed at room temperature for 5 days in a dark place for aging, and then placed in a vacuum mud kneading machine with a vacuum degree of >100 kPa for mud kneading; (4) Put the mixed mud after the first mud kneading into a plastic bag and place it at room temperature for 12 days in a dark place for secondary aging; (5) Add the remaining raw materials to the mixed mud after secondary aging, mix well, and put it into a vacuum mud kneading machine with a vacuum degree of more than 150 kPa for secondary mud kneading; (6) Make the clay into a body, dry it, apply a layer of transparent glaze, and let it dry; (7) The air-dried green body is placed in a kiln and fired at a staged temperature control process, wherein the staged temperature control process is as follows: a first heating process, raising the temperature to 280°C at a rate of 6°C / min and keeping the temperature for 3 hours; a second heating process, raising the temperature to 1650°C at a rate of 5°C / min, while introducing 5% of the total volume of flue gas in carbon monoxide, and keeping the temperature for 2 hours; a first cooling process, lowering the temperature to below 1200°C at a rate of 12°C / min and while introducing 1.5% of the total volume of flue gas in oxygen; a second cooling process, natural cooling, and obtaining a finished ceramic product.
[0023] Example 3 A process for manufacturing ceramic products from clay material that restores the characteristics of Macang clay, comprising the following steps: (1) Prepare the raw materials according to the formula, including 50 parts of quartz, 40 parts of sericite, 10 parts of plagioclase, 25 parts of kaolinite, 20 parts of muscovite, 2 parts of cobalt oxide, 1 part of strontium carbonate, 2 parts of polystyrene, 2 parts of iron oxide, 4 parts of potassium oxide, 2.5 parts of sodium oxide, and 45 parts of water, for later use. The particle size of quartz is 0.5-2 μm; the particle size of sericite is 0.1-1 μm; the particle size of plagioclase is 1.5-3 μm; the particle size of kaolinite is 3-5 μm, the particle size of muscovite is 2-8 μm; and the particle size of polystyrene is 5-15 μm. (2) Mix quartz, sericite, plagioclase, kaolinite, muscovite and strontium carbonate evenly, pass through a 500-mesh sieve, add 95% water, and stir evenly; (3) The mixed mud is placed in a plastic bag and placed at room temperature for 8 days in a dark place for aging, and then placed in a vacuum mud kneading machine with a vacuum degree of >100 kPa for mud kneading; (4) Put the mixed mud after the first mud kneading into a plastic bag and place it at room temperature for 8 days in a dark place for secondary aging; (5) Add the remaining raw materials to the mixed mud after secondary aging, mix well, and put it into a vacuum mud kneading machine with a vacuum degree of more than 150 kPa for secondary mud kneading; (6) Make the clay into a body, dry it, apply a layer of transparent glaze, and let it dry; (7) The air-dried green body is placed in a kiln and fired at a staged temperature control process, wherein the staged temperature control process is as follows: a first heating process, raising the temperature to 350°C at a rate of 8°C / min and keeping the temperature for 2 hours; a second heating process, raising the temperature to 1700°C at a rate of 6°C / min, while introducing 6% of the total volume of flue gas in carbon monoxide, and keeping the temperature for 1 hour; a first cooling process, lowering the temperature to below 1200°C at a rate of 15°C / min, while introducing 2% of the total volume of flue gas in oxygen; a second cooling process, natural cooling, and obtaining a finished ceramic product.
[0024] Comparative Example 1 A process for manufacturing ceramic products from clay materials, which differs from Example 1 in that cobalt oxide is not added to the raw materials.
[0025] Comparative Example 2 A process for manufacturing ceramic products from clay materials, which differs from Example 1 in that strontium carbonate is not added to the raw materials.
[0026] Comparative Example 3 A process for manufacturing ceramic products from clay materials, which differs from Example 1 in that no polystyrene is added to the raw materials.
[0027] Comparative Example 4 A process for manufacturing ceramic products from clay materials, which differs from Example 1 in that no iron oxide is added to the raw materials.
[0028] Comparative Example 5 A process for manufacturing ceramic products from clay material that restores the characteristics of Macang clay, comprising the following steps: (1) Prepare the raw materials according to the formula, including 40 parts of quartz, 20 parts of sericite, 20 parts of plagioclase, 20 parts of kaolinite, 25 parts of muscovite, 1 part of cobalt oxide, 0.8 parts of strontium carbonate, 3 parts of polystyrene, 2 parts of iron oxide, 2.5 parts of potassium oxide, 4 parts of sodium oxide, and 40 parts of water, for later use. The particle size of quartz is 0.5-2 μm; the particle size of sericite is 0.1-1 μm; the particle size of plagioclase is 1.5-3 μm; the particle size of kaolinite is 3-5 μm, the particle size of muscovite is 2-8 μm; and the particle size of polystyrene is 5-15 μm. (2) After mixing all the raw materials evenly, pass them through a 500-mesh sieve, add water, stir evenly, and place them in a vacuum mud kneading machine with a vacuum degree of >100 kPa for a first mud kneading; (3) The mixed mud is placed in a plastic bag and placed at room temperature for 16 days in a dark place for aging, and then placed in a vacuum mud kneading machine with a vacuum degree of >150 kPa for secondary mud kneading; (4) Make the clay into a body, dry it, apply a layer of transparent glaze, and let it dry; (5) The air-dried green body is loaded into a kiln and fired at a staged temperature control process, wherein the staged temperature control process is as follows: a first heating process, raising the temperature to 300°C at a rate of 5°C / min and keeping the temperature for 2.5 hours; a second heating process, raising the temperature to 1600°C at a rate of 4°C / min, while introducing carbon monoxide in an amount of 4% of the total volume of the flue gas, and keeping the temperature for 1.5 hours; a first cooling process, lowering the temperature to below 1200°C at a rate of 10°C / min, while introducing oxygen in an amount of 1% of the total volume of the flue gas; a second cooling process, natural cooling, and obtaining a finished ceramic product.
[0029] Comparative Example 6 A process for manufacturing ceramic products from clay material that restores the characteristics of Macang clay, comprising the following steps: (1) Prepare the raw materials according to the formula, including 40 parts of quartz, 20 parts of sericite, 20 parts of plagioclase, 20 parts of kaolinite, 25 parts of muscovite, 1 part of cobalt oxide, 0.8 parts of strontium carbonate, 3 parts of polystyrene, 2 parts of iron oxide, 2.5 parts of potassium oxide, 4 parts of sodium oxide, and 40 parts of water, for later use. The particle size of quartz is 0.5-2 μm; the particle size of sericite is 0.1-1 μm; the particle size of plagioclase is 1.5-3 μm; the particle size of kaolinite is 3-5 μm, the particle size of muscovite is 2-8 μm; and the particle size of polystyrene is 5-15 μm. (2) Mix quartz, sericite, plagioclase, kaolinite, muscovite and strontium carbonate evenly, pass through a 500-mesh sieve, add 95% water, and stir evenly; (3) The mixed mud is placed in a plastic bag and placed at room temperature for 6 days in a dark place for aging, and then placed in a vacuum mud kneading machine with a vacuum degree of >100 kPa for mud kneading; (4) Put the mixed mud after the first mud kneading into a plastic bag and place it at room temperature for 10 days in a dark place for secondary aging; (5) Add the remaining raw materials to the mixed mud after secondary aging, mix well, and put it into a vacuum mud kneading machine with a vacuum degree of more than 150 kPa for secondary mud kneading; (6) Make the clay into a body, dry it, apply a layer of transparent glaze, and let it dry; (7) The dried green body is placed in a kiln for firing, wherein the firing temperature is raised to 1600°C at a rate of 4°C / min, and 4% of the total volume of the flue gas is introduced into the kiln for 4 hours; then the temperature is cooled once, and the temperature is reduced to below 1200°C at a rate of 10°C / min, and 1% of the total volume of the flue gas is introduced into the kiln; the temperature is cooled twice, and the product is cooled naturally to obtain a finished ceramic product.
[0030] Comparative Example 7 A process for manufacturing ceramic products from clay material that restores the characteristics of Macang clay, comprising the following steps: (1) Prepare the raw materials according to the formula, including 40 parts of quartz, 20 parts of sericite, 20 parts of plagioclase, 20 parts of kaolinite, 25 parts of muscovite, 1 part of cobalt oxide, 0.8 parts of strontium carbonate, 3 parts of polystyrene, 2 parts of iron oxide, 2.5 parts of potassium oxide, 4 parts of sodium oxide, and 40 parts of water, for later use. The particle size of quartz is 0.5-2 μm; the particle size of sericite is 0.1-1 μm; the particle size of plagioclase is 1.5-3 μm; the particle size of kaolinite is 3-5 μm, the particle size of muscovite is 2-8 μm; and the particle size of polystyrene is 5-15 μm. (2) Mix quartz, sericite, plagioclase, kaolinite, muscovite and strontium carbonate evenly, pass through a 500-mesh sieve, add 95% water, and stir evenly; (3) The mixed mud is placed in a plastic bag and placed at room temperature for 6 days in a dark place for aging, and then placed in a vacuum mud kneading machine with a vacuum degree of >100 kPa for mud kneading; (4) Put the mixed mud after the first mud kneading into a plastic bag and place it at room temperature for 10 days in a dark place for secondary aging; (5) Add the remaining raw materials to the mixed mud after secondary aging, mix well, and put it into a vacuum mud kneading machine with a vacuum degree of more than 150 kPa for secondary mud kneading; (6) Make the clay into a body, dry it, apply a layer of transparent glaze, and let it dry; (7) The air-dried green body is placed in a kiln and fired under staged temperature control, wherein the staged temperature control process is as follows: heating up once, raising the temperature to 300°C at a rate of 5°C / min, and keeping the temperature for 2.5 hours; heating up twice, raising the temperature to 1600°C at a rate of 4°C / min, while introducing carbon monoxide in an amount of 4% of the total volume of flue gas, and keeping the temperature for 1.5 hours; and cooling naturally to obtain a finished ceramic product.
[0031] The appearance, thermal stability and water absorption of the ceramics prepared in Examples 1-3 and Comparative Examples 1-7 were tested, and the results are shown in Table 1. The thermal stability test method is as follows: take a ceramic product as a sample, place it at 280°C for 5 hours, take out the sample after the insulation and quickly put it into water at a temperature of 20°C within 15 seconds, immerse it in water for 10 minutes, then take out the sample, wipe it with a cloth, apply red ink, check for cracks, and recheck it after 24 hours. The fewer cracks, the better the thermal stability of the sample; the water absorption test method is as follows: take 5 ceramic products as samples, wash and dry them, weigh them separately, then separate the samples and place them in distilled water, boil them for 3 hours, then fish out the samples, wipe off the water attached to the surface of the samples with a cloth saturated with water, and quickly weigh them separately, and then calculate the water absorption of each sample by the formula, calculate the average water absorption of the 5 samples, that is, the water absorption of the ceramic product, and the lower the water absorption, the better the water resistance of the sample.
[0032] Table 1 Performance test results
[0033] From the results in Table 1, it can be seen that the porcelain products made with the clay formula and manufacturing process of the present invention have good thermal stability and appropriate water absorption. At the same time, the surface is goose egg green with a small amount of bulging and brown eyes. There is natural and obvious flint red at the junction of the bottom and the glaze surface, showing the typical characteristics of Macang clay ceramic products.
[0034] In Comparative Example 1, cobalt oxide is not added and its color is too white; in Comparative Example 2, strontium carbonate is not added, and no bulging or brown eyes appear; in Comparative Example 3, although no polypropylene is added, which has little effect on the appearance, its water absorption is small and the texture is too dense, and it cannot reflect the characteristic of more pores in Macang earthenware products compared with kaolin; in Comparative Example 4, no additional iron oxide is added, and its iron content is insufficient, and the obtained flint red is not obvious; in Comparative Example 5, only one aging is used, although the appearance is not novel, the performance of the product is reduced; in Comparative Example 6, no staged heating is performed, and the temperature rises too fast, polypropylene and strontium carbonate decompose quickly, and the healing is slow, resulting in more pores and affecting water resistance; in Comparative Example 7, the temperature is directly lowered naturally once, and the cooling is slow. After the carbon dioxide after the decomposition of strontium carbonate is released and the glaze surface heals, brown eyes cannot be formed.
[0035] Finally, it should be emphasized that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various changes and modifications. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A clay material that restores the characteristics of Macang soil, It is characterized in that The mud material includes the following raw material components in parts by weight: 40-50 parts of quartz, 20-40 parts of sericite, 10-20 parts of plagioclase, 20-25 parts of kaolinite, 20-25 parts of muscovite, 1-2 parts of cobalt oxide, 0.5-1 parts of strontium carbonate, 2-5 parts of polystyrene, 1-2 parts of iron oxide, 2.5-4 parts of potassium oxide, 2.5-4 parts of sodium oxide, and 35-45 parts of water.
2. The clay material that restores the characteristics of Macakura soil according to claim 1, It is characterized in that The particle size of the quartz is 0.5-2 μm; the particle size of the sericite is 0.1-1 μm; and the particle size of the plagioclase is 1.5-3 μm.
3. The clay material that restores the characteristics of Macakura soil according to claim 1, It is characterized in that The particle size of the kaolinite is 3-5 μm, and the particle size of the muscovite is 2-8 μm.
4. The clay material that restores the characteristics of Macakura soil according to claim 3, It is characterized in that The particle size of the polystyrene is 5-15 μm.
5. A process for manufacturing ceramic products using a clay material that restores the characteristics of Macakura soil as claimed in any one of claims 1 to 4, It is characterized in that The following steps are involved: (1) Prepare all raw materials according to the recipe and set aside; (2) Mix quartz, sericite, plagioclase, kaolinite, muscovite and strontium carbonate evenly, pass through a 500-mesh sieve, add 95% water, and stir evenly; (3) The mixed mud is aged once, and then placed in a vacuum mud kneading machine for mud kneading; (4) Secondary aging of the mixed mud after the first mud kneading; (5) Add the remaining raw materials to the mixed mud after secondary aging, mix well and put it into a vacuum mud kneading machine for secondary mud kneading; (6) Make the clay into a body, dry it, apply a layer of transparent glaze, and let it dry; (7) The dried green body is placed in a kiln and the firing temperature is controlled in stages. After the firing is completed and the green body is cooled, a finished ceramic product is obtained.
6. The process according to claim 5, It is characterized in that In step (3), the primary aging process is as follows: the mixed mud is placed in a plastic bag and placed at room temperature in a dark place for 5-8 days; the vacuum degree of the mud kneading is greater than 100 kPa.
7. The process according to claim 5, It is characterized in that In step (4), the secondary aging process is as follows: the mixed mud after the first mud kneading is placed in a plastic bag under light-shielded conditions at room temperature for 8-12 days; in step (5), the vacuum degree of the mud kneading is >150 kPa.
8. The process according to claim 5, It is characterized in that In step (7), the process of staged temperature control is as follows: first heating, raising the temperature to 280-350°C at a rate of 5-8°C / min, and keeping it warm for 2-3h; second heating, raising the temperature to 1600-1700°C at a rate of 4-6°C / min, and keeping it warm for 1-2h; first cooling, lowering the temperature to below 1200°C at a rate of 10-15°C / min; second cooling, natural cooling.
9. The process according to claim 8, It is characterized in that In the secondary heating stage, 4-6% of the total volume of the flue gas is carbon monoxide introduced simultaneously; in the primary cooling stage, 1-2% of the total volume of the flue gas is oxygen introduced simultaneously.
10. A ceramic with reduced Makura clay properties manufactured by the process according to any one of claims 5 to 9.
Citation Information
Cited By
High-whiteness unglazed ice jade porcelain and preparation method thereof
CN120004509A