Dry vibration material binding agent and preparation method thereof

By using combination agents of components such as silica sol, phenolic resin and amino compounds in dry vibrating materials, the problems of low compressive strength and flexural strength are solved, and higher fire resistance is achieved and the needs of high-temperature industries are met.

CN119039012AActive Publication Date: 2024-11-29LANGFANG SENDE TECH CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411222153.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-29
Estimated Expiration
2044-09-02

AI Technical Summary

Technical Problem

The compressive strength and flexural strength of dry vibrating materials are low, making it difficult to meet the performance requirements of high-temperature industries for refractory materials.

Method used

A dry vibrating material bonding agent, including silica sol, phenolic resin, amino compounds and surfactants, is used to increase the stability of the compounding of phenolic resin and silica sol by adding compatible agents, thereby enhancing the strength of the binder.

Benefits of technology

It significantly improves the flexural strength and pressure resistance of dry vibrating materials, improves the service life and construction performance of the materials, and meets industrial production needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of refractory materials, and provides a dry vibration material binding agent and a preparation method thereof.The binding agent is prepared from, by weight, 40-50 parts of silica sol, 3-8 parts of compatilizer, 10-15 parts of phenolic resin and 0.2-0.4 part of surfactant, and the compatilizer comprises an amino compound. According to the technical scheme, the problems of low compression strength and breaking strength of the dry vibration material in the prior art are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of refractory materials, and in particular to a dry vibrating material binder and a preparation method thereof. Background Art

[0002] With the continuous development of high temperature industries such as metallurgy, chemical industry, and building materials, the performance requirements for refractory materials are becoming higher and higher. Dry vibrating material is a loose refractory material composed of refractory aggregate, powder, binder and admixture. When in use, the material is compacted by vibration, thereby obtaining good construction performance and use performance.

[0003] Among them, the binder plays a vital role, which can bind the refractory aggregate and the powder together to form a whole with certain strength and stability. Therefore, it is necessary to provide a binder that can further improve the compressive strength and flexural strength of the dry vibrating material. Summary of the invention

[0004] The invention provides a dry vibrating material binder and a preparation method thereof, which solves the problem of low compressive strength and flexural strength of dry vibrating material in the related art.

[0005] The technical solution of the present invention is as follows: The present invention provides a dry vibration material binder, which comprises the following raw materials in parts by weight: 40-50 parts of silica sol, 3-8 parts of a compatibilizer, 10-15 parts of a phenolic resin, and 0.2-0.4 parts of a surfactant, wherein the compatibilizer comprises an amino compound.

[0006] As a further technical solution, the SiO2 content in the silica sol is 40wt%.

[0007] As a further technical solution, the free phenol content in the phenolic resin is less than 12wt%, and the solid content is greater than 75wt%.

[0008] As a further technical solution, the amino compound includes one or more of 3-bis(2-hydroxyethyl)amino-2-hydroxypropanesulfonic acid and 7-amino-4-hydroxy-2-naphthalenesulfonic acid.

[0009] As a further technical solution, the amino compound consists of 3-bis(2-hydroxyethyl)amino-2-hydroxypropanesulfonic acid and 7-amino-4-hydroxy-2-naphthalenesulfonic acid.

[0010] When the amino compound in the present invention consists of 3-bis(2-hydroxyethyl)amino-2-hydroxypropanesulfonic acid and 7-amino-4-hydroxy-2-naphthalenesulfonic acid, the prepared binder can better improve the flexural strength and compressive strength of the dry vibration material.

[0011] As a further technical solution, the mass ratio of the 3-bis(2-hydroxyethyl)amino-2-hydroxypropanesulfonic acid to the 7-amino-4-hydroxy-2-naphthalenesulfonic acid is 1:1.

[0012] As a further technical solution, the raw materials of the binder also include polyacrylamide.

[0013] As a further technical solution, the molecular weight of the polyacrylamide is 14 to 20 million.

[0014] As a further technical solution, the molecular weight of the polyacrylamide is 18 million.

[0015] As a further technical solution, the mass ratio of the 3-bis(2-hydroxyethyl)amino-2-hydroxypropanesulfonic acid, 7-amino-4-hydroxy-2-naphthalenesulfonic acid and polyacrylamide is 1:1:1.

[0016] As a further technical solution, the mass ratio of the compatibilizer to the silica sol is 3~8:40.

[0017] As a further technical solution, the mass ratio of the compatibilizer to the silica sol is 4~7:40.

[0018] As a further technical solution, the mass ratio of the compatibilizer to the silica sol is 1:8.

[0019] As a further technical solution, the surfactant is a non-ionic surfactant.

[0020] As a further technical solution, the nonionic surfactant includes one or two of polyethylene glycol, alkylphenol polyoxyethylene ether, and block polyether.

[0021] The present invention also proposes a method for preparing a dry vibration material binder, comprising the following steps: mixing the raw materials uniformly to obtain the dry vibration material binder.

[0022] The working principle and beneficial effects of the present invention are: In the present invention, the binder used for the dry vibration material is an organic-inorganic binder. Through the synergistic effect of the organic and inorganic binders, the dry vibration material can have good fluidity during the processing process, and the dry vibration material has higher strength and better thermal shock resistance, which prolongs the service life of the material and meets the needs of industrial production; wherein the inorganic binder is silica sol, and the organic binder is phenolic resin. The mixture of phenolic resin and silica sol can improve the strength of the binder, but when the phenolic resin and silica sol are compounded for use at the same time, there will be a problem of poor stability, thereby affecting the bonding strength of the phenolic resin and silica sol, resulting in a decrease in the flexural strength and compressive strength of the dry vibration material. The addition of a compatibilizer can improve the stability of the phenolic resin and silica sol when they are compounded for use, and further improve the flexural strength and compressive strength of the dry vibration material. DETAILED DESCRIPTION

[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] In the following examples and comparative examples: Silica sol: SiO2 content 40wt%; Phenolic resin 213: free phenol content <12wt%, solid content >75wt%, Zhengzhou Hengtong Chemical Co., Ltd.

[0025] Example 1 A method for preparing a dry vibrating material binder comprises the following steps: After 40 parts of silica sol, 3 parts of compatibilizer, 10 parts of phenolic resin 213 and 0.2 parts of polyethylene glycol 600 are uniformly mixed to obtain a dry vibration material binder; wherein the compatibilizer is 3-bis(2-hydroxyethyl)amino-2-hydroxypropanesulfonic acid.

[0026] Example 2 A method for preparing a dry vibrating material binder comprises the following steps: After 45 parts of silica sol, 4 parts of compatibilizer, 12 parts of phenolic resin 213 and 0.3 parts of polyethylene glycol 600 are uniformly mixed to obtain a dry vibration material binder: wherein the compatibilizer is 3-bis(2-hydroxyethyl)amino-2-hydroxypropanesulfonic acid.

[0027] Example 3 A method for preparing a dry vibrating material binder comprises the following steps: After 50 parts of silica sol, 5 parts of compatibilizer, 15 parts of phenolic resin 213 and 0.4 parts of polyethylene glycol 600 are uniformly mixed to obtain a dry vibration material binder; wherein the compatibilizer is 3-bis(2-hydroxyethyl)amino-2-hydroxypropanesulfonic acid.

[0028] Example 4 The only difference between this embodiment and embodiment 1 is that the compatibilizer is 7-amino-4-hydroxy-2-naphthalenesulfonic acid.

[0029] Example 5 The only difference between this embodiment and embodiment 1 is that the compatibilizer is 3-bis(2-hydroxyethyl)amino-2-hydroxypropanesulfonic acid and 7-amino-4-hydroxy-2-naphthalenesulfonic acid in a mass ratio of 1:1.

[0030] Example 6 The only difference between this embodiment and embodiment 1 is that the compatibilizer is 3-bis(2-hydroxyethyl)amino-2-hydroxypropanesulfonic acid, 7-amino-4-hydroxy-2-naphthalenesulfonic acid and polyacrylamide (molecular weight 14 million) in a mass ratio of 1:1:1.

[0031] Example 7 The only difference between this embodiment and embodiment 6 is that the amount of the compatibilizer added is 8 parts.

[0032] Example 8 The only difference between this embodiment and embodiment 6 is that the amount of the compatibilizer added is 4 parts.

[0033] Example 9 The only difference between this embodiment and embodiment 6 is that the amount of the compatibilizer added is 5 parts.

[0034] Example 10 The only difference between this embodiment and embodiment 6 is that the amount of the compatibilizer added is 7 parts.

[0035] Embodiment 11 The only difference between this embodiment and embodiment 9 is that the molecular weight of polyacrylamide is 18 million.

[0036] Example 12 The only difference between this embodiment and embodiment 9 is that the molecular weight of the polyacrylamide is 20 million.

[0037] Comparative Example 1 The only difference between this comparative example and Example 1 is that 3-bis(2-hydroxyethyl)amino-2-hydroxypropanesulfonic acid is not added.

[0038] Test example The properties of the binders prepared in Examples 1 to 12 and Comparative Example 1 were determined by the following specific determination methods: The raw materials of dry vibration material were prepared according to the mass ratio of 6:1:5:2 of magnesia-chrome sand (particle size of 0-5mm), fused magnesia sand (particle size of 0-5mm), binder and borax (particle size of 0-2mm). The raw materials of dry vibration material were mixed evenly and then vibrated into shape. The materials were baked at 200°C and demolded to obtain dry vibration material. The flexural strength of dry vibration material was determined according to GB / T 3002-2017 "Test method for high temperature flexural strength of refractory materials", and the compressive strength of dry vibration material was determined according to GB / T 34218-2017 "Test method for high temperature compressive strength of refractory materials". The test results are shown in Table 1.

[0039] Table 1 Performance test results of the binder in Examples 1 to 12 and Comparative Example 1

[0040] Compared with Example 1, Comparative Example 1 does not add 3-bis(2-hydroxyethyl)amino-2-hydroxypropanesulfonic acid. As a result, the flexural strength and compressive strength of Example 1 are higher than those of Comparative Example 1, indicating that the addition of amino compounds in the present invention can improve the flexural strength and compressive strength of dry vibration materials.

[0041] Compared with Example 1, the compatibilizer in Example 4 is 7-amino-4-hydroxy-2-naphthalenesulfonic acid, and the compatibilizer in Example 5 is 3-bis(2-hydroxyethyl)amino-2-hydroxypropanesulfonic acid and 7-amino-4-hydroxy-2-naphthalenesulfonic acid. As a result, the flexural strength and compressive strength of Example 5 are higher than those of Example 1 and Example 4, indicating that the simultaneous addition of 3-bis(2-hydroxyethyl)amino-2-hydroxypropanesulfonic acid and 7-amino-4-hydroxy-2-naphthalenesulfonic acid can further improve the flexural strength and compressive strength of the dry vibration material.

[0042] Compared with Example 5, the compatibilizer of Example 6 also includes polyacrylamide. As a result, the flexural strength and compressive strength of Example 6 are higher than those of Example 5, indicating that when the compatibilizer is 3-bis(2-hydroxyethyl)amino-2-hydroxypropanesulfonic acid, 7-amino-4-hydroxy-2-naphthalenesulfonic acid and polyacrylamide, the flexural strength and compressive strength of the dry vibration material can be further improved.

[0043] Compared with Example 6, Examples 7 to 10 change the amount of compatibilizer added. As a result, the flexural strength and compressive strength of Examples 8 to 10 are higher than those of Examples 6 to 7, indicating that when the mass ratio of the compatibilizer to the silica sol is 4 to 7:40, the flexural strength and compressive strength of the dry vibrating material can be better improved.

[0044] Compared with Example 9, Examples 11-12 change the molecular weight of polyacrylamide. As a result, the flexural strength and compressive strength of Example 11 are higher than those of Example 9 and Example 12, indicating that when the molecular weight of polyacrylamide is 1800, the flexural strength and compressive strength of the dry vibration material can be further improved.

[0045] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A dry vibrating material binder, characterized in that: The binder comprises the following raw materials in parts by weight: 40-50 parts of silica sol, 3-8 parts of a compatibilizer, 10-15 parts of a phenolic resin, and 0.2-0.4 parts of a surfactant, wherein the compatibilizer comprises an amino compound.

2. A dry vibration material binder according to claim 1, characterized in that: The amino compound includes one or more of 3-bis(2-hydroxyethyl)amino-2-hydroxypropanesulfonic acid and 7-amino-4-hydroxy-2-naphthalenesulfonic acid.

3. A dry vibration material binder according to claim 2, characterized in that: The amino compound consists of 3-bis(2-hydroxyethyl)amino-2-hydroxypropanesulfonic acid and 7-amino-4-hydroxy-2-naphthalenesulfonic acid.

4. A dry vibration material binder according to claim 1, characterized in that: The raw materials of the binder also include polyacrylamide.

5. A dry vibration material binder according to claim 4, characterized in that: The molecular weight of the polyacrylamide is 14 to 20 million.

6. A dry vibration material binder according to claim 1, characterized in that: The mass ratio of the compatibilizer to the silica sol is 3-8:

40.

7. A dry vibration material binder according to claim 1, characterized in that: The surfactant is a nonionic surfactant.

8. A dry vibration material binder according to claim 7, characterized in that: The nonionic surfactant includes one or two of polyethylene glycol, alkylphenol polyoxyethylene ether and block polyether.

9. A dry vibration material binder according to claim 3, characterized in that: The mass ratio of the 3-bis(2-hydroxyethyl)amino-2-hydroxypropanesulfonic acid to the 7-amino-4-hydroxy-2-naphthalenesulfonic acid is 1:

1.

10. The method for preparing a dry vibration material binder according to any one of claims 1 to 9, characterized in that: The following steps are involved: After the raw materials are uniformly mixed, a dry vibration material binder is obtained.

Citation Information

Patent Citations

  • Silanol-based bicomponent waterborne polyurethane wood adhesive and preparation method thereof

    CN107446538A

  • Sulfamate polymer dispersant and preparation method thereof, and applications in ceramic slurries

    CN110028642A

  • High-strength adhesive taking inorganic matters as main components and preparation method thereof

    CN112552014A

  • Boiler lining thermal insulation material and preparation method thereof

    CN115196982A

  • Adhesion agent for casting blast furnace hearth and use method of adhesion agent

    CN115636670A