Self-assembled cuprous sulfide nanocrystal energetic compound as well as preparation method and application thereof

By preparing cuprous sulfide nanocrystals via a solvothermal method and then self-assembling them to coat energetic materials, the problem of high laser ignition threshold was solved, and low-power-density laser ignition was achieved, making it suitable for miniaturized weapons.

CN119039095APending Publication Date: 2024-11-29INST OF CHEM MATERIAL CHINA ACADEMY OF ENG PHYSICS

Patent Information

Application Number
CN202411174022.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing energetic materials have high laser ignition thresholds, making it difficult to meet the application requirements of miniaturized weapons, and traditional photothermal conversion materials have insufficient photothermal conversion efficiency.

Method used

Oleic acid/oleylamine-stabilized cuprous sulfide nanocrystals were prepared by a solvothermal method. They formed a core-shell structure through self-assembly, which coated the surface of energetic materials, enhancing light absorption and photothermal conversion efficiency and reducing the thermal decomposition temperature peak.

Benefits of technology

It significantly reduces the laser ignition threshold of energetic materials, enabling low-power-density laser ignition, which is suitable for miniaturized weapons and has a simple manufacturing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039095A_ABST
    Figure CN119039095A_ABST
Patent Text Reader

Abstract

The invention discloses a self-assembled cuprous sulfide nanocrystalline energetic compound as well as a preparation method and application thereof, and relates to the technical field of energetic materials. Firstly, cuprous sulfide dispersion liquid is prepared, then cuprous sulfide is self-assembled on the surface of an energetic material, and the self-assembled cuprous sulfide nanocrystalline energetic compound is obtained. The compound has a typical core-shell structure, the shell structure is self-assembled cuprous sulfide nanocrystals, the content of the self-assembled cuprous sulfide nanocrystals is 1%-5% based on the total mass of 100%, the core structure is an energetic material, and the content of the energetic material is 95%-99%; the cuprous sulfide nanocrystal energetic material can be applied to laser ignition, the near-infrared light absorption and photothermal conversion efficiency of the energetic material are enhanced through the cuprous sulfide nanocrystal on the surface layer, the effect of remarkably reducing the laser ignition threshold value is achieved, the cuprous sulfide nanocrystal energetic material has wide application prospects in the field of laser initiating explosive device charging, and the preparation process is simple and convenient and easy to implement.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of energetic materials, and in particular to a general preparation method of a self-contained cuprous sulfide nanocrystal energetic composite and its application in reducing the laser ignition threshold in the laser ignition of energetic materials and realizing low-power density laser ignition of semiconductor lasers. Background Art

[0002] Laser ignition means that energetic materials burn or explode under the action of lasers, and the conversion of electrical energy into chemical energy is completed through light energy. Since the energetic materials are not in direct contact with the power source and are not affected by electromagnetic waves, this is an advanced pyrotechnic technology that is safer and more reliable than traditional ignition methods. Most energetic materials have no or weak absorption in the near-infrared band, resulting in a laser ignition threshold that is too high to be directly ignited. Currently, the laser ignition threshold is mainly reduced by doping light-absorbing sensitizing materials into high explosives. In 2009, BP Aduev et al. of the Russian Academy of Sciences found that after mixing nickel-carbon composites (5wt.%) into pentaerythritol tetranitrate (PETN), its laser ignition threshold was reduced to 5J / cm 2 [Combust.Explos.Shock Waves, 2009, 45, 59], in 2015, Fang.X et al. from Cranfield University, UK, doped carbon black (5wt.%) in 1,1-diamino-2,2-dinitroethylene (FOX-7) and realized laser ignition of it, with an ignition threshold of 104W / cm 2 [J.Hazard.Mater.,2015,285,375]. In 2018, Jixiang Bo et al. from the Institute of Chemical Materials, China Academy of Engineering Physics, doped nano-aluminum powder (5wt.%) with hexanitrohexaazaisowurtzitane (Cl-20) to increase its minimum ignition energy from 100 J / cm 2 Reduced to 2J / cm 2 [Propellants, Explos., Pyrotech., 2018, 43, 1210]. Although adding carbon black or nano-aluminum powder can make some energetic materials ignite by near-infrared laser, the laser energy required for ignition is still too high. It is not only difficult to meet the needs of fiber optic energy transmission, but also requires a large solid laser, which limits the application of laser pyrotechnics in miniaturized weapons. Therefore, breaking through the bottleneck of high laser ignition threshold is the most worthy research hotspot in the field of energetic materials in the next few years. In recent years, metal sulfide (selenide) compounds have attracted great attention from researchers in various fields as photothermal conversion materials (Table 1). This photothermal conversion phenomenon originates from the surface plasmon effect. In addition, due to oleylamine or oleic acid as ligands, the nanomaterials prepared by the solvothermal method have the property of orderly self-assembly when the solvent evaporates [Nature 2010, 466, 474].

[0003] Table 1: Photothermal conversion efficiency (η) and laser emission wavelength of common photothermal conversion materials

[0004] Nanomaterials η(%) Wavelength (nm) References <![CDATA[Cu 2-X With]]> 65 808 Adv.Mater.2016,28,8927 <![CDATA[Au@Cu 2-X S]]> 59 808 Adv.Mater.2016,28,3094 <![CDATA[Bi 2 With 3 ]]> 51 808 ACS Nano 2016,10,11145 <![CDATA[Cu 7 S 4 ]]> 49 808 Small 2015,11,4183 <![CDATA[MoS 2 ]]> 44 808 ACS Nano 2016,10,11000 <![CDATA[Ag 2 S]]> 35 785 ACS Nano 2017,11,1848 <![CDATA[Cu 1.8 S / MoS 2 ]]> 33 980 Adv.Funct.Mater.2017,27,1605592 <![CDATA[Fe 3 A 4 @With 2-X S]]> 16 980 J.Am.Chem.Soc.2013,135,8571 Summary of the invention

[0005] The purpose of the present invention is to reduce the laser ignition threshold of energetic materials, overcome the difficulty of laser ignition of energetic materials, provide a general preparation method of self-assembled cuprous sulfide nanocrystal energetic complex and apply it to the laser ignition system. First, oleic acid / oleylamine stabilized cuprous sulfide nanocrystals are prepared by solvothermal method. Since the long alkyl chain of oleic acid / oleylamine has hydrophobic properties, the cuprous sulfide nanocrystals have good dispersibility in non-polar solvents such as cyclohexane, toluene or chloroform. When the low boiling point solvent evaporates, the cuprous sulfide nanocrystals can self-assemble on the surface of the energetic material to form a core-shell structure, thereby achieving all-round coating and modification of the surface of the energetic material, increasing the light absorption intensity and photothermal conversion efficiency of the energetic material in the near-infrared band, and making it heat up higher under laser irradiation; at the same time, cuprous ions catalyze and reduce the thermal decomposition temperature peak of the energetic material, making it easier to ignite. The self-assembly coating of cuprous sulfide nanocrystals solves the common technical problems of high laser ignition threshold and difficult laser ignition of energetic materials.

[0006] In order to achieve the above-mentioned purpose of the invention, the present invention adopts the following preparation method, and the prepared self-loaded cuprous sulfide nanocrystal energetic composite has a typical core-shell structure, the shell structure is self-loaded cuprous sulfide nanocrystals, with a total mass of 100%, and a content of 1% to 5%, and the core structure is an energetic material, with a content of 95% to 99%.

[0007] The term "nanocrystal" is short for nanoscale crystals.

[0008] The term "self-assembly" refers to the spontaneous formation of ordered structures by basic building blocks (nanocrystals) and aggregation on the surface of energetic materials.

[0009] The method for preparing a self-contained cuprous sulfide nanocrystal energetic composite comprises the following steps:

[0010] (1) Preparation of cuprous sulfide dispersion

[0011] (1.1) preparing a sulfur precursor reaction solution: dissolving a sulfur-containing element reagent in 1-octadecene to obtain a sulfur precursor reaction solution;

[0012] Optionally, the sulfur-containing element reagent is selected from one of sublimated sulfur and thiourea;

[0013] Optionally, the ratio of the molar amount of the sulfur-containing reagent to the volume of 1-octadecene is: 10-30 mmol: 160 mL. Under this ratio, the sulfur-containing reagent can be fully dissolved in 1-octadecene under certain conditions; 1-octadecene serves as a high boiling point reaction buffer;

[0014] Optionally, the sulfur-containing reagent and 1-octadecene are mixed and then heated to above 180° C. to promote the dissolution of the sulfur-containing reagent in 1-octadecene, which is beneficial to improving the dissolution efficiency and solubility of the sulfur-containing reagent in 1-octadecene; such as dissolving at a temperature of 180° C., 190° C., 200° C., 210° C., 220° C., etc.;

[0015] Optionally, stirring is used during the dissolution process to promote the dispersion and dissolution of the sulfur-containing reagent in 1-octadecene;

[0016] Generally, stirring at a temperature above 180°C for about 30 minutes can promote the full dissolution of the sulfur-containing reagent and 1-octadecene in a ratio of 10-30mmol:160mL, so that the sulfur-containing reagent can be fully dissolved in a shorter time; shortening the stirring time may result in a small amount of sulfur-containing reagent not being fully dissolved, and significantly extending the stirring time does not have a better promoting effect on the full dissolution of the sulfur-containing reagent. Extended stirring leads to reduced process efficiency. Therefore, it is recommended that the stirring time be controlled within 30 to 45 minutes;

[0017] Optionally, the dissolution process is protected by argon, that is, the sulfur-containing reagent and 1-octadecene are placed in an argon environment and dissolved in this environment to avoid the influence of water and oxygen in the air on the raw sulfur-containing reagent and 1-octadecene, such as oxidation (especially under high temperature conditions) and the introduction of impurities.

[0018] Optionally, the heating method is oil bath heating;

[0019] The above are some good methods or conditions that can be selected when preparing the sulfur precursor reaction solution. However, a relatively simple operation method is: weigh 10-30 mmol of the sulfur-containing element reagent and add it to 160 mL of 1-octadecene, stir and disperse it, heat it to 180°C, and fully dissolve it for 30 minutes under argon protection to obtain a sulfur precursor reaction solution.

[0020] (1.2) preparing a copper precursor reaction solution: dissolving a copper element-containing reagent in a mixed solvent consisting of oleylamine and oleic acid;

[0021] Optionally, the copper-containing reagent is selected from cuprous chloride, cupric chloride, copper nitrate, and cuprous bromide;

[0022] Optionally, in the mixed solvent composed of oleylamine and oleic acid, the volume ratio of oleylamine to oleic acid is 14-18:20, preferably 16:20; oleylamine and oleic acid serve as ligands to stabilize the cuprous sulfide nanocrystals;

[0023] Optionally, the ratio of the molar amount of the copper-containing reagent to the volume of the mixed solvent composed of oleylamine and oleic acid is 10-30mmol:34-38mL; under this ratio, the copper-containing reagent can be fully dissolved in the mixed solvent composed of oleylamine and oleic acid under certain conditions;

[0024] Optionally, the copper-containing reagent is mixed with a mixed solvent consisting of oleylamine and oleic acid and then heated to above 130° C. to promote the dissolution of the copper-containing reagent in the mixed solvent consisting of oleylamine and oleic acid, which is beneficial to improving the dissolution efficiency and solubility of the copper-containing reagent in the mixed solvent consisting of oleylamine and oleic acid; such as dissolving at a temperature of 130° C., 140° C., 150° C., 160° C., 170° C., etc.;

[0025] Generally, stirring at a temperature above 130°C for about 30 minutes can promote the full dissolution of the copper-containing reagent and the mixed solvent composed of oleylamine and oleic acid in a dosage ratio of 10-30mmol:34-38mL, so that the copper-containing reagent can be fully dissolved in a shorter time; the optional stirring rate is ≤1500rpm; shortening the stirring time may cause a small amount of copper-containing reagent to be not fully dissolved, and significantly extending the stirring time does not have a better promoting effect on the full dissolution of the copper-containing reagent. Extended stirring leads to reduced process efficiency. Therefore, it is recommended that the stirring time be controlled at 30-45 minutes; adjusting the stirring rate affects the dissolution rate to a certain extent. However, in order to fully dissolve in a short time and be easy to achieve, it is recommended to select a stirring rate less than or equal to 1500rpm, and the preferred stirring rate is 500-1200rpm;

[0026] Optionally, the dissolution process is protected by argon, that is, the copper-containing reagent and the mixed solvent composed of oleylamine and oleic acid are placed in an argon environment and dissolved in this environment to avoid the influence of the air environment on the raw copper-containing reagent and the mixed solvent composed of oleylamine and oleic acid, such as oxidation (especially under high temperature conditions) and the introduction of impurities;

[0027] Optionally, the heating method is oil bath heating;

[0028] The above are some good methods or conditions that can be selected when preparing the copper precursor reaction solution. However, a relatively simple operation method is: weigh 10-30 mmol of the copper element reagent, add it to 16 mL of oleylamine and 20 mL of oleic acid, and heat it to 130°C and fully dissolve it under argon protection for 30 minutes.

[0029] As an optional method, the reaction of step (1.1) and step (1.2) can be completed in a double-row tube reaction system, and the reaction liquid needs to be dehydrated and deoxygenated and protected with inert gas to prevent high-temperature oxidation.

[0030] (1.3) mixing the copper precursor reaction liquid and the sulfur precursor reaction liquid to react with each other to form cuprous sulfide nanocrystals, collecting the cuprous sulfide nanocrystal precipitate in the reaction liquid by centrifugation after the reaction is completed, and dispersing the precipitate in a non-polar solvent to obtain a cuprous sulfide dispersion;

[0031] Optionally, the molar ratio of the sulfur-containing reagent in the copper precursor reaction solution to the copper-containing reagent in the sulfur precursor reaction solution is 1:1;

[0032] Optionally, the copper precursor reaction liquid is added to the sulfur precursor reaction liquid, or the sulfur precursor reaction liquid is added to the copper precursor reaction liquid. However, since the volume of the sulfur precursor reaction liquid is significantly larger than that of the copper precursor reaction liquid, it is better to add the copper precursor reaction liquid to the sulfur precursor reaction liquid.

[0033] Optionally, the copper precursor reaction liquid and the sulfur precursor reaction liquid are mixed and heated to above 180° C. to promote the reaction between the two to generate cuprous sulfide nanocrystals; such as reacting at a temperature of 180° C., 190° C., 200° C., 210° C., 220° C., etc.; the heating method may be an oil bath, but is not limited thereto;

[0034] Reaction time and temperature affect the synthesis rate of cuprous sulfide nanocrystals. A reaction temperature above 180°C shortens the time for complete reaction while promoting the formation of cuprous sulfide nanocrystals. It is recommended to control the reaction time to 30 to 45 minutes under this temperature condition to complete the reaction quickly. Constant temperature reaction can be selected, but it is not required. However, constant temperature is a relatively simple operation mode, so it is easier to achieve by constant temperature reaction.

[0035] Optionally, after the reaction is completed and the mixture is naturally cooled to room temperature, the cuprous sulfide nanocrystals are collected from the reaction solution by centrifugation. After the reaction solution is centrifuged, the cuprous sulfide nanocrystals are precipitated, the supernatant is discarded, and the precipitate is collected to obtain the cuprous sulfide nanocrystals. Other conventional separation methods may be used instead of centrifugation.

[0036] Optionally, the non-polar solvent is a low boiling point solvent, and the non-polar solvent is selected from one or a mixture of cyclohexane, toluene, and chloroform; the non-polar solvent plays a role in dispersing the cuprous sulfide nanocrystals to prevent the aggregation of nanomaterials from affecting subsequent self-assembly. Therefore, the amount of the non-polar solvent is not critical, but for ease of operation and economy, it is recommended to use 20 to 200 mL of non-polar solvent to disperse the cuprous sulfide nanocrystals prepared by using 10-30 mmol of sulfur-containing reagent, preferably 40 to 100 mL of non-polar solvent.

[0037] Optionally, the reaction process is protected by argon, that is, the copper precursor reaction liquid and the sulfur precursor reaction liquid are placed in an argon environment, and the reaction is carried out in this environment to synthesize cuprous sulfide nanocrystals, thereby avoiding the influence of the air environment on the raw materials, such as oxidation (especially under high temperature conditions) and the introduction of impurities.

[0038] The above are some of the better methods or conditions that can be selected when preparing cuprous sulfide dispersion, but a relatively simple operation method is:

[0039] After the copper precursor reaction liquid and the sulfur precursor reaction liquid are fully dissolved, the copper precursor reaction liquid is quickly added to the sulfur precursor reaction liquid, and the reaction is carried out at a constant temperature of 180°C for 30 minutes under the protection of argon. After the reaction is completed, it is naturally cooled to room temperature, and the cuprous sulfide nanocrystals are collected by centrifugation. After the supernatant reaction liquid is discarded, the precipitate can be well dispersed in a non-polar solvent, and the obtained cuprous sulfide dispersion is used for the formation of the self-assembled structure in the next step;

[0040] (2) Self-assembly of cuprous sulfide on the surface of energetic materials

[0041] Adding energetic materials to the cuprous sulfide dispersion to disperse the energetic materials in the cuprous sulfide dispersion, and allowing the non-polar solvent in the cuprous sulfide dispersion to completely evaporate, thereby obtaining a self-assembled cuprous sulfide nanocrystal energetic composite;

[0042] Optionally, when adding the energetic material to the cuprous sulfide dispersion, the mass concentration of the energetic material is controlled to be 0.1-1.0 g / L, so that more cuprous sulfide is self-assembled on the surface of the energetic material; preferably 0.5 g / L, which can not only make more cuprous sulfide self-assembled on the surface of the energetic material, but also make the cuprous sulfide self-assembled on the surface of the energetic material uniform;

[0043] Optionally, in order to make the energetic material uniformly dispersed in the cuprous sulfide dispersion, conventional dispersion methods such as ultrasonic dispersion and stirring dispersion can be used, among which ultrasonic dispersion is preferred (the preferred vibration frequency is 10 to 40 kHz, which is relatively energy-saving when the purpose is achieved);

[0044] Optionally, during the dispersion process, a fume hood is opened to accelerate the volatilization of the non-polar solvent, thereby improving efficiency; during the volatilization of the non-polar solvent, the cuprous sulfide nanocrystals gradually self-assemble onto the surface of the energetic material, and when the solvent is completely volatilized, the cuprous sulfide nanocrystals completely self-assemble onto the surface of the energetic material, thereby obtaining the self-assembled cuprous sulfide nanocrystal energetic complex of the present invention.

[0045] Optionally, the solvent is evaporated and the cuprous sulfide self-assembly shell is coated on the surface of the energetic material at room temperature, and the solvent evaporation time is 10 to 30 minutes. Increasing the temperature can accelerate the solvent evaporation and thus shorten the time required for self-assembly, but this requires heating equipment and energy, and is dangerous because the solution contains energetic materials. In addition, too fast evaporation of the solvent affects the uniformity of the self-assembled shell to a certain extent. Lowering the temperature is unnecessary, which results in a too long evaporation time and a significant reduction in preparation efficiency. Therefore, it is recommended to complete the solvent evaporation at room temperature.

[0046] The energetic material is any one of ammonium perchlorate (AP), hexanitrohexaazaisopentazolane (Cl-20), 5,5'-biquatrazol-1,1'-dioxydihydroxyamine (TKX-50), and 2,2',3,3'-tetranitro-1,1'-diamino-5,5'-biimidazole (DATNBI).

[0047] The present invention provides the use of the self-assembled cuprous sulfide nanocrystal energetic composite in laser ignition, using a near-infrared (wavelength of 808nm, 980nm or 1064nm) semiconductor laser for ignition, with a power density of 2 to 80W / cm 2 , the irradiation time is 100ms. Since the ignition delay time of the composite is less than 100ms, ignition can be ensured and easy to operate under this irradiation time.

[0048] In the above application, the self-assembled cuprous sulfide nanocrystal energetic composite used preferably contains 95% to 99% energetic material and 1% to 5% cuprous sulfide nanocrystals based on 100% total mass.

[0049] Compared with the prior art, the present invention has at least the following beneficial effects:

[0050] First, cuprous sulfide nanocrystals have a larger molar extinction coefficient (1.15*10 8 M - 1 cm -1 ) and photothermal conversion efficiency (71%), and can reduce the thermal decomposition temperature peak of some energetic materials (AP, DATNBI); secondly, the solvent-driven self-assembly process can comprehensively coat the energetic materials, which is better than the coating effect of simple mixing and is beneficial to the comprehensive heating of the energetic materials under laser irradiation.

[0051] The self-assembled cuprous sulfide nanocrystal energetic composite was applied to laser ignition, which can significantly reduce the energetic laser threshold and better sensitize the laser sensitivity of energetic materials under the condition of lower cuprous sulfide nanocrystal coating amount. For pure AP, Cl-20, TKX-50 or DATNBI, the maximum power density of semiconductor laser (80W / cm 2 ) could not be ignited successfully. Only the AP coated with cuprous sulfide nanocrystals could achieve laser ignition. The minimum laser ignition energy of AP coated with 5% cuprous sulfide nanocrystals was 2W / cm 2 , at the maximum laser ignition energy of 80W / cm 2 The ignition delay time is 3ms; the minimum laser ignition energy of DATNBI coated with 1% cuprous sulfide nanocrystals is 64W / cm 2 , at the maximum laser ignition energy of 80W / cm 2 The ignition delay time is 24ms. The invention has a wide application prospect in laser explosive charge, and the preparation process is simple and easy to implement. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] In order to more clearly illustrate the technical solutions in the embodiments of this application document or the prior art, the following briefly introduces the drawings required for use in the description of the embodiments or the prior art.

[0053] Figure 1 The photograph of cuprous sulfide nanocrystals dispersed in cyclohexane (25 mg / mL) involved in the present invention (left) and the transmission electron microscopy characterization of cuprous sulfide nanocrystals (right).

[0054] Figure 2 This is a photo of the preparation process of the self-assembled cuprous sulfide nanocrystal energetic composite (above) and a schematic diagram of the assembly process (below).

[0055] Figure 3 These are the scanning electron microscopy results of self-assembled cuprous sulfide nanocrystal energetic composites.

[0056] Figure 4 1 and 2 are the laser ignition results of the self-contained cuprous sulfide nanocrystal energetic composites, wherein (a) is the laser ignition result of the composite prepared in Example 1, (b) is the laser ignition result of the composite prepared in Example 2, (c) is the laser ignition result of the composite prepared in Example 3, and (d) is the laser ignition result of the composite prepared in Example 4.

[0057] Obviously, the accompanying drawings are only references to some embodiments in the present application document. For those skilled in the art, other accompanying drawings can be obtained based on these accompanying drawings without creative work. DETAILED DESCRIPTION

[0058] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0059] Example 1

[0060] Step 1: 0.64 g (20 mmol) of sublimed sulfur was dissolved in 160 ml of 1-octadecene, the oil bath was heated to 180° C., and stirred at 900 rpm for 30 minutes to fully dissolve the sublimed sulfur. During this period, argon was introduced into the reaction solution as a protective gas to prevent the reagent from being oxidized. 2.00 g (20 mmol) of cuprous chloride was weighed and dissolved in 16 ml of oleylamine and 20 ml of oleic acid. The oil bath was heated to 130° C., and stirred at 900 rpm for 30 minutes to fully dissolve the cuprous chloride. Argon was introduced into the reaction solution as a protective gas to prevent the reagent from being oxidized. After the cuprous chloride was completely dissolved, the mixed solution was quickly added to the sublimed sulfur / 1-octadecene mixed solution, and the mixture was kept at 180° C. for full reaction for 30 minutes, during which argon was continuously introduced. After the reaction is completed, the mixture is cooled to room temperature naturally, and the cuprous sulfide precipitate is collected by centrifugation. The supernatant reaction solution is discarded, and 40 mL of cyclohexane is added to redisperse the cuprous sulfide nanocrystals to obtain a cuprous sulfide nanocrystal dispersion with a mass solubility of about 25 mg / mL. Figure 1 (Left) As shown. Transmission electron microscopy characterization of cuprous sulfide nanocrystals Figure 1 (right) shown.

[0061] Step 2: Weigh 20 mL of the cuprous sulfide nanocrystal dispersion obtained in step 1 (containing 500 mg of cuprous sulfide nanocrystals and 20 mL of cyclohexane) and add it to a beaker containing 10 g of AP. Figure 2 As shown, cyclohexane was dispersed ultrasonically and volatilized naturally in a fume hood. After 20 minutes, the cyclohexane was completely volatilized, and the AP composite coated with self-loaded cuprous sulfide in the present invention was obtained. The obtained composite was characterized by scanning electron microscopy as shown in FIG. Figure 3 As shown, the surface of the obtained AP is coated with self-assembled cuprous sulfide.

[0062] Finally, 20 mg of the AP composite coated with self-assembled cuprous sulfide was placed loosely on the laser ignition board and ignited under a semiconductor laser with a wavelength of 1064 nm. The results showed that the minimum laser ignition energy of 5% by mass ammonium perchlorate coated with cuprous sulfide nanocrystals was 2 W / cm 2 , at the maximum laser ignition energy of 80W / cm 2 The ignition delay time is 3ms and the flame color is orange ( Figure 4 a), compared with AP raw materials (at maximum laser ignition energy 80W / cm 2The self-assembly of cuprous sulfide nanocrystals can significantly reduce the laser ignition threshold of AP.

[0063] Example 2

[0064] Step 1: Take 0.64g (20mmol) of sublimed sulfur and dissolve it in 160ml of 1-octadecene, heat the oil bath to 180℃, stir and dissolve at 900rpm for 30 minutes, pass argon into the reaction solution as a protective gas to prevent the reagent from being oxidized, weigh 3.41g (20mmol) of cupric chloride and dissolve it in 16ml of oleylamine and 20ml of oleic acid, heat the oil bath to 130℃, stir and dissolve at 900rpm for 30 minutes, pass argon into the reaction solution as a protective gas to prevent the reagent from being oxidized, wait for the cupric chloride to be completely dissolved, quickly add the sublimed sulfur / 1-octadecene mixture to the mixture, keep the temperature at 180℃ and fully react for 30 minutes, and continue to pass argon during the reaction. After the reaction is completed, cool naturally to room temperature, collect the cuprous sulfide precipitate by centrifugation, discard the supernatant reaction solution, add 40mL of cyclohexane to redisperse the cuprous sulfide nanocrystals, and obtain a cuprous sulfide nanocrystal dispersion with a mass solubility of about 25mg / mL.

[0065] Step 2: Weigh 10 mL of the cuprous sulfide nanocrystal dispersion obtained in step 1 (containing 250 mg of cuprous sulfide nanocrystals and 10 mL of cyclohexane), add it to a beaker containing 10 mL of cyclohexane and 10 g of Cl-20, and ultrasonically disperse and naturally volatilize the cyclohexane in a fume hood. After 20 minutes, the cyclohexane is completely evaporated to obtain the Cl-20 complex coated with self-contained cuprous sulfide in the present invention.

[0066] Finally, 20 mg of the self-assembled cuprous sulfide-coated Cl-20 composite was placed loosely on a laser ignition plate and ignited under a 1064 nm wavelength semiconductor laser. The results showed that the minimum laser ignition energy of 2.5% mass ratio of cuprous sulfide nanocrystal-coated Cl-20 was 48 W / cm 2 , at the maximum laser ignition energy of 80W / cm 2 The ignition delay time is 82ms and the flame color is bright white ( Figure 4 b), compared to Cl-20 raw material (at maximum laser ignition energy 80 W / cm 2 The self-assembly of cuprous sulfide nanocrystals can significantly reduce the laser ignition threshold of Cl-20.

[0067] Example 3

[0068] Step 1: Take 1.52g (20mmol) of thiourea and dissolve it in 160ml of 1-octadecene, heat the oil bath to 180℃, stir and dissolve at 900rpm for 30 minutes, pass argon into the reaction solution as a protective gas to prevent the reagent from being oxidized, weigh 2.87g (20mmol) of cuprous bromide and dissolve it in 16ml of oleylamine and 20ml of oleic acid, heat the oil bath to 130℃, stir and dissolve at 900rpm for 30 minutes, pass argon into the reaction solution as a protective gas to prevent the reagent from being oxidized, wait for cuprous bromide to be completely dissolved, quickly add the mixture to thiourea / 1-octadecene mixture, keep the temperature at 180℃ and fully react for 30 minutes, and pass argon. After the reaction is completed, cool naturally to room temperature, collect the cuprous sulfide precipitate by centrifugation, discard the supernatant reaction solution, add 40mL of cyclohexane to redisperse the cuprous sulfide nanocrystals, and obtain a cuprous sulfide nanocrystal dispersion with a mass solubility of about 25mg / mL.

[0069] Step 2: Weigh 20 mL of the cuprous sulfide nanocrystal dispersion obtained in step 1 (containing 500 mg of cuprous sulfide nanocrystals and 10 mL of cyclohexane), add it to a beaker containing 10 g of TKX-50, and disperse it ultrasonically in a fume hood and naturally evaporate the cyclohexane. After 20 minutes, the cyclohexane evaporates completely, and the self-loaded cuprous sulfide-coated TKX-50 composite of the present invention is obtained.

[0070] Finally, 20 mg of the self-assembled cuprous sulfide-coated TKX-50 composite was placed loosely on the laser ignition board and ignited under a 1064 nm wavelength semiconductor laser. The results showed that the minimum laser ignition energy of 5% mass ratio cuprous sulfide nanocrystal-coated TKX-50 was 32 W / cm 2 , at the maximum laser ignition energy of 80W / cm 2 The ignition delay time is 5ms and the flame color is orange ( Figure 4 c), compared to TKX-50 raw material (at maximum laser ignition energy 80W / cm 2 The self-assembly of cuprous sulfide nanocrystals can significantly reduce the laser ignition threshold of TKX-50.

[0071] Example 4

[0072] Step 1: Take 1.52g (20mmol) of thiourea and dissolve it in 160ml of 1-octadecene, heat the oil bath to 180℃, stir and dissolve at 900rpm for 30 minutes, pass argon into the reaction solution as a protective gas to prevent the reagent from being oxidized, weigh 4.83g (20mmol) of copper nitrate and dissolve it in 16ml of oleylamine and 20ml of oleic acid, heat the oil bath to 130℃, stir and dissolve at 900rpm for 30 minutes, pass argon into the reaction solution as a protective gas to prevent the reagent from being oxidized, wait for the copper nitrate to be completely dissolved, quickly add the thiourea / 1-octadecene mixture to the mixture, keep the temperature at 180℃ and fully react for 30 minutes, and pass argon. After the reaction is completed, cool naturally to room temperature, collect the cuprous sulfide precipitate by centrifugation, discard the supernatant reaction solution, add 40mL of cyclohexane to redisperse the cuprous sulfide nanocrystals, and obtain a cuprous sulfide nanocrystal dispersion with a mass solubility of about 25mg / mL.

[0073] Step 2: Weigh 4 mL of the cuprous sulfide nanocrystal dispersion obtained in step 1 (containing 100 mg of cuprous sulfide nanocrystals and 4 mL of cyclohexane), add it to a beaker containing 16 mL of cyclohexane and 10 g of DATNBI, and disperse it ultrasonically in a fume hood and volatilize the cyclohexane naturally. After 20 minutes, the cyclohexane is completely evaporated to obtain the self-contained cuprous sulfide-coated DATNBI complex of the present invention.

[0074] Finally, 20 mg of the self-assembled cuprous sulfide-coated DATNBI composite was placed loosely on a laser ignition board and ignited under a 1064 nm wavelength semiconductor laser. The results showed that 1% by mass cuprous sulfide nanocrystal-coated DATNBI was applied to laser ignition, and the minimum laser ignition energy was 64 W / cm 2 , at the maximum laser ignition energy of 80W / cm 2 Under the condition, the ignition delay time is 24ms, and the flame color is orange ( Figure 4 d), compared with DATNBI raw material (at maximum laser ignition energy 80W / cm 2 The self-assembly of cuprous sulfide nanocrystals can significantly reduce the laser ignition threshold of DATNBI.

[0075] Although the present invention is described herein with reference to the illustrative embodiments of the present invention, it should be understood that those skilled in the art can design many other modifications and implementations, which will fall within the scope and spirit of the principles disclosed in the present application. More specifically, within the scope disclosed in the present application, multiple variations and improvements can be made to the components and / or layout of the subject combination layout. In addition to the variations and improvements made to the components and / or layout, other uses will also be apparent to those skilled in the art.

Claims

1. A self-contained cuprous sulfide nanocrystal energetic composite, It is characterized in that It has a core-shell structure, the shell structure is self-loaded cuprous sulfide nanocrystals, and the core structure is an energetic material; based on its total mass being 100%, the content of the shell structure is 1% to 5%, and the content of the core structure is 95% to 99%.

2. The self-contained cuprous sulfide nanocrystal energetic composite according to claim 1, It is characterized in that The energetic material is any one of AP, Cl-20, TKX-50, and DATNBI.

3. A method for preparing a self-contained cuprous sulfide nanocrystal energetic composite, It is characterized in that The following steps are involved: (1) Preparation of cuprous sulfide dispersion (1.1) preparing a sulfur precursor reaction solution: dissolving a sulfur-containing element reagent in 1-octadecene to obtain a sulfur precursor reaction solution; (1.2) preparing a copper precursor reaction solution: dissolving a copper element-containing reagent in a mixed solvent consisting of oleylamine and oleic acid; (1.3) mixing the copper precursor reaction liquid and the sulfur precursor reaction liquid to react with each other to form cuprous sulfide nanocrystals, collecting the cuprous sulfide nanocrystal precipitate in the reaction liquid by centrifugation after the reaction is completed, and dispersing the precipitate in a non-polar solvent to obtain a cuprous sulfide dispersion; (2) Self-assembly of cuprous sulfide on the surface of energetic materials The energetic material is added into the cuprous sulfide dispersion so that the energetic material is dispersed in the cuprous sulfide dispersion and the non-polar solvent in the cuprous sulfide dispersion is completely volatilized to obtain a self-assembled cuprous sulfide nanocrystal energetic composite.

4. The method for preparing the self-contained cuprous sulfide nanocrystal energetic composite according to claim 3, It is characterized in that The sulfur-containing element reagent is selected from sublimed sulfur or thiourea, and the ratio of the molar amount of the sulfur-containing element reagent to the volume of 1-octadecene is: 10-30mmol:160mL.

5. The method for preparing the self-contained cuprous sulfide nanocrystal energetic composite according to claim 3, It is characterized in that The copper-containing reagent is selected from one of cuprous chloride, cupric chloride, cupric nitrate and cuprous bromide. The ratio of the molar amount of the copper-containing reagent to the volume of a mixed solvent consisting of oleylamine and oleic acid is 10-30mmol:34-38mL. In the mixed solvent consisting of oleylamine and oleic acid, the volume ratio of oleylamine to oleic acid is 14-18:

20.

6. The method for preparing the self-contained cuprous sulfide nanocrystal energetic composite according to claim 4, It is characterized in that In step (1.1), the sulfur-containing reagent is mixed with 1-octadecene and then heated to above 180° C. to promote the dissolution of the sulfur-containing reagent in 1-octadecene; in step (1.2), the copper-containing reagent is mixed with a mixed solvent consisting of oleylamine and oleic acid and then heated to above 130° C. to promote the dissolution of the copper-containing reagent in the mixed solvent consisting of oleylamine and oleic acid; in step (1.3), the copper precursor reaction liquid and the sulfur precursor reaction liquid are mixed and then heated to above 180° C. to promote the reaction between the two to generate cuprous sulfide nanocrystals.

7. The method for preparing the self-contained cuprous sulfide nanocrystal energetic composite according to claim 3, It is characterized in that The molar ratio of the sulfur-containing reagent in the copper precursor reaction solution to the copper-containing reagent in the sulfur precursor reaction solution is 1:

1.

8. The method for preparing the self-contained cuprous sulfide nanocrystal energetic composite according to claim 3, It is characterized in that The non-polar solvent is selected from one or a mixture of cyclohexane, toluene and chloroform; step (1.1), step (1.2) and step (1.3) are all protected by argon gas, and stirring is used to promote the solvent or reaction; ultrasonic dispersion is used in step (2) to disperse the energetic material in the cuprous sulfide dispersion.

9. The method for preparing the self-contained cuprous sulfide nanocrystal energetic composite according to claim 3, It is characterized in that The energetic material is AP, Cl-20, TKX-50 or DATNBI.

10. Use of the self-contained cuprous sulfide nanocrystal energetic composite according to claim 1 or 2, It is characterized in that Application in laser ignition, using near-infrared semiconductor laser for ignition, power density is 2~80W / cm 2 .

Citation Information

Patent Citations

  • Silicon dioxide coated cuprous sulfide nanometer crystal core-shell structure and preparation method thereof

    CN109568581A

  • Preparation method of precious metal / copper sulfide core-shell structure nanocrystalline

    CN110918017A

  • Regulation and control method of Cu2-xS nanosheet crystal structure

    CN111498895A

  • Method of reducing laser ignition energy

    CN112707774A

  • Preparation method and application of aluminum powder surface atomic layer deposition CuOx modification layer

    CN112708870A

Cited By

  • Method for generating in-situ nanocrystalline of powder metallurgy material