Calcium magnesium acetate prepared from phosphate tailings as well as preparation method and application of calcium magnesium acetate

By using high-temperature calcination and acetic acid acid hydrolysis processes, the activity of calcium oxide and magnesium oxide in phosphorus tailings is improved, and a highly active calcium magnesium acetate de-icing agent is prepared. This solves the problems of insufficient yield and high cost in existing technologies, and realizes the efficient recycling and industrial application of phosphorus tailings.

CN119039133APending Publication Date: 2024-11-29ZHENGZHOU UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411167975.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing technologies for preparing calcium magnesium acetate (CMA) de-icing agents from phosphate tailings suffer from low leaching rates of calcium oxide and magnesium oxide, resulting in insufficient CMA production, high production costs, and a failure to effectively increase the added value of phosphate tailings recycling, making industrial application difficult.

Method used

By reacting phosphate tailings with acetic acid at high temperature, the activity of calcium oxide and magnesium oxide is improved. Highly active calcium magnesium acetate is prepared by using acetic acid acid hydrolysis and evaporation crystallization processes. This simplifies the process, reduces costs, and improves the recovery rate and economic added value of phosphate tailings.

Benefits of technology

It significantly improves the yield and recovery rate of CMA, reduces production costs, solves the environmental hazards and safety risks caused by the accumulation of phosphate tailings, provides high-grade phosphate rock raw materials, lays the foundation for the production of high value-added phosphate chemical products, and is suitable for industrial promotion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039133A_ABST
    Figure CN119039133A_ABST
Patent Text Reader

Abstract

The invention provides calcium magnesium acetate prepared from phosphate tailings as well as a preparation method and application of the calcium magnesium acetate. According to the preparation method, low-grade phosphate tailings are mainly used as raw materials, and magnesium calcium acetate with magnesium acetate tetrahydrate and calcium acetate hemihydrate as main components is prepared through high-temperature calcination and acetic acid hydrolysis; therefore, the acidolysis reaction rate is increased, the whole production period of calcium magnesium acetate is remarkably shortened, and the production efficiency of calcium magnesium acetate is improved; the yield of calcium magnesium acetate is obviously improved, the dosage of acetic acid is reduced, and the production cost is greatly reduced; therefore, the calcium magnesium acetate crop snow-melting agent prepared by the invention has the characteristics of high quality, low cost, wide application and the like. In addition, the preparation method also improves the grade of P2O5 in the phosphate tailings, so that the low-grade phosphate tailings are converted into the raw material high-grade phosphorite which can be used for directly generating phosphorus chemical products with high additional value. Therefore, the preparation method can improve the economic added value of the phosphate tailings, and is suitable for industrial popularization and application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of waste resource utilization, and in particular to calcium magnesium acetate prepared from phosphate tailings, and a preparation method and application thereof. Background Art

[0002] Phosphate tailings are solid wastes generated during the beneficiation process of phosphate ore. Every ton of phosphate concentrate will produce 0.3-0.5 tons of phosphate tailings. As the mining volume of phosphate ore continues to increase, the discharge of phosphate tailings is also growing rapidly. A large amount of phosphate tailings are piled up in tailings ponds and farmland, which not only occupies a large amount of land resources, but also wastes mineral resources, and also causes serious environmental pollution and safety hazards. Therefore, providing an effective comprehensive utilization method for phosphate tailings and turning them into treasure is an inevitable choice for the sustainable and healthy development of the domestic phosphorus chemical industry.

[0003] The main mineral components of phosphate tailings are dolomite, apatite, etc., which contain valuable elements such as calcium, magnesium, iron, aluminum, and manganese in addition to phosphorus, and are secondary resources rich in calcium and magnesium and low in phosphorus. Domestic researchers have conducted a lot of research on the recycling of calcium and magnesium elements with surplus value in phosphate tailings. The existing technology usually processes phosphate tailings, separates calcium and magnesium therein, and prepares calcium carbonate, magnesium hydroxide, and magnesium oxide products, which provides basic information for the comprehensive utilization of phosphate tailings. However, the existing methods usually fail to achieve industrialization and effectively achieve the purpose of comprehensive utilization of associated resources due to factors such as high energy consumption and high cost of the production process.

[0004] Calcium magnesium acetate (CMA), a mixture of calcium acetate and magnesium acetate, is a new type of environmentally friendly deicing agent. Compared with the existing chloride-type deicing agents, which are used in an application ratio of more than 90%, it has the advantages of low corrosivity, biodegradability, and little harm to plants. However, the existing CMA uses dolomite and acetic acid as raw materials, and the production cost is too high, which limits the promotion and use of CMA deicing agents. It is generally only used in special occasions such as airports and highways. Therefore, the development of a cheap production process of calcium magnesium acetate has become the key to popularizing the environmentally friendly deicing agent calcium magnesium acetate.

[0005] To this end, Wang Baoming's research group at Zhengzhou University provided a process for preparing calcium magnesium acetate de-icing agent by using acetic acid to hydrolyze phosphate tailings (Li Mengyu, Tang Jianwei, Liu Yong, et al. Research on the process of preparing calcium magnesium acetate de-icing agent by using acetic acid to hydrolyze phosphate tailings [J]. Inorganic Salt Industry, 2024, 56(01): 73-80). The preparation process directly hydrolyzes phosphate tailings with acetic acid solution to obtain acid hydrolysis slag and acid hydrolysis liquid. The mass fraction of P2O5 in the acid hydrolysis slag is increased to 25.91%. The acid hydrolysis liquid is evaporated and crystallized after adjusting the pH to obtain CMA. All indicators of CMA meet the requirements of GB / T 23851-2017 "De-icing Agents". It is an environmentally friendly de-icing agent with low corrosiveness, biodegradability and excellent ice and snow melting performance. However, the leaching rates of calcium oxide and magnesium oxide in the above process are both lower than 80%, which affects the full recycling of phosphate tailings and the output of CMA. In addition, although the acid-lysis slag can be used as medium-grade phosphate ore, it cannot be directly applied to the production of high-value-added phosphorus chemical products and needs to be processed before use. Therefore, the above process of preparing calcium-magnesium acetate snow-melting agent by using acetic acid to acid-lyze phosphate tailings has the problem that the added value of recycling phosphate tailings needs to be further improved. Summary of the invention

[0006] In view of this, the first object of the present invention is to provide a method for preparing CMA using phosphate tailings as raw materials. This method uses dolomite-rich phosphate tailings as raw materials, and reacts with acetic acid after high-temperature calcination, which greatly increases the CMA output and reduces production costs; at the same time, it increases the grade of P2O5 in the phosphate tailings, providing direct raw materials for the production of high-added phosphorus chemical products. Therefore, the above-mentioned CMA preparation method can not only convert low-grade phosphate tailings into high-grade phosphate ore, but also make the prepared snow-melting agent CMA high-quality and low-cost, suitable for wide use, thereby effectively improving the economic added value of phosphate tailings recycling, which is conducive to industrial promotion and application. In order to achieve the above purpose, the technical solution provided by the present invention specifically includes: a method for preparing calcium magnesium acetate using phosphate tailings, comprising the steps of:

[0007] High-temperature calcination: First, the phosphorus tailings are subjected to high-temperature calcination treatment to obtain calcined activated phosphorus tailings;

[0008] Acetic acid acidolysis: uniformly mixing the acetic acid solution and the calcined activated phosphate tailings to carry out leaching reaction, filtering, and obtaining an acidolysis solution and an acidolysis residue;

[0009] Purification and crystallization: The acid hydrolyzate is subjected to evaporation and crystallization treatment, and then dried to obtain CMA.

[0010] The content of P2O5 in the phosphorus tailings is preferably no more than 15%. The phosphorus tailings are preferably dolomite-rich phosphorus tailings, whose main phase composition includes dolomite CaMg(CO3)2, fluoroapatite Ca5(PO4)3F, quartz SiO2, and the main elements contained are Ca, Mg, P, Si, Al, F, C, etc. Among them, the content of dolomite in the phosphorus tailings is preferably 65%-75%. The main chemical components of the phosphorus tailings include CaO, MgO, CO2, P2O5, SiO2, etc. The particle size of the phosphorus tailings is preferably 40-240μm.

[0011] The main purpose of the high-temperature calcination is to extract calcium and magnesium elements from the phosphate tailings, and effectively improve the activity of CaO and MgO that can react with acetic acid, so as to improve the CMA yield, the recovery rate of the phosphate tailings and the economic added value. In order to achieve this purpose, the step of high-temperature calcination specifically includes: heating the phosphate tailings to 800-900℃ at a heating rate of 5-20℃ / min and calcining for 20-50min to obtain the calcined activated phosphate tailings; wherein the physical composition of the calcined activated phosphate tailings includes CaO, MgO, Ca5(PO4)3F, SiO2, etc.; the main chemical components include CaO, MgO, P2O5, SiO2, etc., and the content of P2O5 is higher than that of the original uncalcined phosphate tailings. Preferably, the particle size of the calcined activated phosphate tailings is 5-45μm.

[0012] During the high-temperature calcination process, it is necessary to control the calcination temperature, calcination time, heating rate and other parameters to ensure that the CaMg(CO3)2 in the phosphate tailings is basically completely decomposed to generate MgO and CaO, and the Ca5(PO4)3F therein does not react, and MgO and CaO have high reactivity, and the increase in temperature activates the lattice of CaO and MgO, and the lattice volume expands due to the intensification of thermal vibration, stretching the interatomic bond length. However, as the temperature continues to rise, the crystals of CaO and MgO gradually develop completely, the crystals gradually stabilize, and the activity tends to be flat or even reduced. The better activity allows it to fully react in the subsequent experimental steps.

[0013] Different heating rates will affect the time required for the heating stage, and thus affect the weight loss rate of the phosphate tailings, and the activity of CaO and MgO. If the heating rate is too fast, the heating time in the early heating stage will be reduced, and the heat absorbed by the phosphate tailings will be reduced. Therefore, in the early stage of calcination, the phosphate tailings will not be decomposed thoroughly, and the content of CaO and MgO produced by decomposition will be insufficient, and the overall activity will be low; if the heating rate is too slow, it will take a long time and the economic cost will be high; so it is limited to 10-20℃ / min.

[0014] Among them, "acetic acid" in the present invention refers to pure glacial acetic acid, and "acetic acid solution" refers to an aqueous solution containing pure glacial acetic acid. During the acetic acid acidolysis process, MgO and CaO in the calcined activated phosphate tailings can react with acetic acid, and calcium and magnesium are leached into the acidolysis solution in the form of ions; the Ca5(PO4)3F therein does not react with acetic acid, and is eventually enriched in the acidolysis slag in the form of precipitation, so that the P2O5 content therein is greatly increased, thereby upgrading the low-grade phosphate tailings to high-grade phosphate ore. Acetic acid reacts with calcium oxide and magnesium oxide in the calcined phosphate tailings to generate calcium acetate and magnesium acetate, and the main ion reaction equations that occur are as follows:

[0015] CaO + 2CH3COOH = Ca 2+ +2CH3COO - +H2O (1);

[0016] MgO+2CH3COOH=Mg 2+ +2CH3COO - +H2O (2).

[0017] Therefore, the main purpose of the acetic acid hydrolysis step is to ensure that the MgO and CaO in the calcined activated phosphate tailings are fully neutralized with acetic acid, and calcium acetate and magnesium acetate are formed, so as to improve the final yield of CMA, the recovery rate of phosphate tailings and the economic added value. Specifically, the acetic acid hydrolysis step includes: under stirring, the acetic acid solution and the calcined activated phosphate tailings react at room temperature for 15-40 minutes, and filter to obtain the acid hydrolysis solution and acid hydrolysis slag. Among them, the main chemical components of the acid hydrolysis solution include: calcium acetate and magnesium acetate; the main phase components of the acid hydrolysis slag are Ca5(PO4)3F (fluoroapatite) and SiO2 (quartz); the particle size is preferably 3-45μm. The stirring speed is preferably 350-450r / min; the room temperature is preferably 15-35°C, more preferably 20-30°C; the amount of acetic acid in the acetic acid solution is preferably 89%-106% of the theoretical amount (theoretical amount refers to the calculated value of the acetic acid amount calculated by an ideal chemical reaction); the liquid-to-solid ratio of the acetic solution to the calcined activated phosphate tailings is preferably (6-14):1.

[0018] The main purpose of the purification and crystallization step is to obtain CMA from the acid hydrolysis solution. This method is a prior art and may specifically include: placing the acid hydrolysis solution in a rotary evaporator for evaporation and crystallization, and drying it in an oven when the solution is evaporated to a white viscous state to obtain the CMA snow melting agent.

[0019] The second object of the present invention is to provide a CMA prepared by the above method, which is mainly composed of magnesium acetate tetrahydrate and calcium acetate hemihydrate, and the CMA is weakly alkaline, has low chloride content, low heavy metal content, and has the characteristics of solid dissolution rate greater than 6.0g / min, lower corrosion rate to carbon steel than distilled water, good ice and snow melting effect, and low relative damage rate to plant seeds. In order to distinguish it from other CMA products, the CMA prepared by the above method provided by the present invention is named as Type II CMA.

[0020] Therefore, the third object of the present invention is to provide a use of the above-mentioned type II CMA in preparing a deicing agent.

[0021] Therefore, the present invention uses phosphate tailings as raw materials, and after high-temperature calcination, it is acidolyzed with acetic acid to improve the activity of magnesium oxide and calcium oxide, not only improves the acidolysis reaction rate, but also greatly shortens the acetic acidolysis process time. At the same time, due to the short calcination process time, the entire CMA production cycle is significantly shortened, and the production efficiency of CMA is improved; and the CMA output is significantly increased, the amount of acetic acid is reduced, and the production cost is greatly reduced; the CMA crop snow melting agent has the characteristics of high quality and low price, suitable for wide use, etc.; in addition, at the same time, the entire CMA preparation process is free of waste, which solves the environmental hazards and safety hazards caused by the accumulation of phosphate tailings, improves the grade of P2O5 in phosphate tailings, converts low-grade phosphate tailings into high-grade phosphate ore, and provides direct raw materials for high-added phosphorus chemical products. Therefore, the above-mentioned CMA preparation method achieves the purpose of improving the economic added value of phosphate tailings recycling and utilization, and is suitable for industrial promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 A process flow chart for preparing CMA using phosphate tailings provided in an embodiment of the present invention;

[0023] Figure 2 It is the thermodynamic equilibrium component diagram of calcination of phosphate tailings;

[0024] Figure 3 The graph of the weight loss rate of phosphorus tailings changing with calcination time at different calcination temperatures;

[0025] Figure 4 The curve diagram of the change of CaO activity of phosphate tailings with calcination time at different calcination temperatures;

[0026] Figure 5 The curve diagram of the change of MgO activity of phosphorus tailings with calcination time at different calcination temperatures;

[0027] Figure 6 It is a curve diagram showing the change of weight loss rate of phosphorus tailings with calcination time at different heating rates;

[0028] Figure 7 The curve diagram of the change of CaO activity of phosphate tailings with calcination time at different heating rates;

[0029] Figure 8 The curve diagram of the change of MgO activity of phosphorus tailings with calcination time at different heating rates;

[0030] Fig. 9 This is the effect of acetic acid dosage on calcium and magnesium leaching rates;

[0031] Fig.10 This is the effect of liquid-solid ratio on calcium and magnesium leaching rate during acetic acid hydrolysis;

[0032] Fig.11 This is the effect of acetic acid hydrolysis reaction time on calcium and magnesium leaching rates;

[0033] Fig.12 The XRD spectrum of the acid-decomposed slag obtained under the optimal process conditions provided by the embodiment of the present invention;

[0034] Fig.13 The SEM image of the acid-decomposed slag obtained under the optimal process conditions provided by the embodiment of the present invention;

[0035] Fig.14 A particle size distribution diagram of the acid-hydrolyzed slag obtained under the optimal process conditions provided by an embodiment of the present invention;

[0036] Fig.15 A photograph of type II CMA prepared under optimal process conditions provided in an embodiment of the present invention;

[0037] Fig.16 The XRD patterns of three CMA de-icing agents are shown below;

[0038] Fig.17 The SEM image of type II CMA prepared under the optimal process conditions provided in the embodiment of the present invention;

[0039] Fig.18 A mapping diagram of a type II CMA prepared under optimal process conditions provided by an embodiment of the present invention;

[0040] Fig.19 Infrared spectra of different CMA snow melting agents;

[0041] Fig. 20 This is a graph showing the snow-melting and ice-melting capabilities of four types of snow-melting agents. DETAILED DESCRIPTION

[0042] The technical solution of the present invention is further described in detail below through specific implementation methods.

[0043] The terms used in the present invention are all commonly used in the field. The raw materials, equipment, preparation processes, test methods, etc. used are all prior art in the field unless otherwise specified. The reagents and products used are also commercially available. The sources and trade names of the reagents used, as well as the components thereof, are indicated when they first appear.

[0044] The solutions used in the following tests were:

[0045] Acetic acid solution: The acetic acid content in the solution is calculated based on the content of CaO, MgO, and Ca5(PO4)3F in the phosphate tailings to obtain the amount of glacial acetic acid required for the complete reaction of a certain mass of phosphate tailings.

[0046] The measurement methods of the parameters or indicators involved in the following tests are as follows:

[0047] MgO activity: Referring to standard YB / 4019-2020, the hydration method was used to determine the content of active magnesium oxide in calcined phosphate tailings.

[0048] CaO activity: Referring to standard YB / 105-2014, the activity of calcium oxide in calcined phosphate tailings is expressed by the number of milliliters of 4 mol / L hydrochloric acid consumed in 10 minutes.

[0049] The leaching rates of CaO and MgO in phosphate tailings are determined according to GB / T 1871.4-1995 “Volumetric method for determination of calcium oxide content in phosphate ore and concentrate”.

[0050] P2O5 content: According to the national standard GB / T 1817.4-1995, the quinoline phosphomolybdic acid weight method (arbitration method) is used to determine the phosphorus pentoxide content in phosphate rock.

[0051] The test methods for the solid dissolution rate, pH, carbon steel corrosion rate, relative damage rate of plant seeds, chloride content and heavy metal content of deicing agents all refer to the standard GB / T 23851-2017.

[0052] The de-icing ability was evaluated by a modified version of the SHRP method: 56 mL of distilled water was poured into a 150 mm diameter culture dish, placed in a high-low temperature alternating humidity test chamber at -10 °C for 12 hours, and an ice sample with a thickness of 3.175 mm was prepared for use; 1.795 g of de-icing agent that had been placed in the high-low temperature alternating humidity test chamber was weighed, evenly spread on the ice surface, and then returned to the test chamber. The culture dish was taken out at 10, 20, 30, 40, 50, and 60 minutes, the ice surface was tilted, and the melted snow water was extracted with a syringe, and the volume was measured and poured back.

[0053] See also Figure 1 The embodiment of the present invention provides a method for preparing CMA using phosphate tailings, comprising:

[0054] 1. High temperature calcination

[0055] First, the phosphate tailings with a particle size of 42.603-236.288 μm are placed in a muffle furnace, and the phosphate tailings are heated to 850°C at a heating rate of 20°C / min and calcined for 30 minutes to obtain the calcined activated phosphate tailings. The main phase composition of the phosphate tailings includes dolomite CaMg(CO3)2, fluoroapatite Ca5(PO4)3F, and quartz SiO2, and the main elements contained are Ca, Mg, P, Si, Al, F, C, etc. The phosphate tailings are further quantitatively analyzed according to the current relevant national standards. The main chemical composition analysis of the phosphate tailings is shown in Table 1.

[0056] Table 1 Main chemical components of phosphate tailings

[0057]

[0058] 1.1 Thermodynamic mechanism of calcination of phosphate tailings

[0059] The thermodynamic calculation software HSC Chemistry 6.0 was used to simulate the calcination process of phosphorus tailings, analyze the thermodynamic reaction equilibrium during the calcination process of phosphorus tailings, study the thermodynamic mechanism, and provide theoretical support for subsequent experiments. Figure 2 shown.

[0060] from Figure 2 It can be seen that CaMg(CO3)2 in the phosphate tailings is first decomposed into CaCO3 and MgCO3 by heat. The generated MgCO3 begins to decompose at about 220℃ and completely decomposes at about 660℃ to generate MgO and CO2. CaCO3 begins to decompose at about 600℃ and decomposes completely at about 1200℃ to generate CaO and CO2. The decomposition temperature of Ca5(PO4)3F is much higher than that of CaMg(CO3)2. It begins to decompose at about 1000℃ to generate Ca3(PO4)2 and CaF2, and decomposes completely at about 2300℃. Therefore, the calcination temperature has an important influence on the composition of the calcined activated phosphate tailings.

[0061] The study found that the parameters such as calcination temperature, calcination time and heating rate have an important influence on the reactivity of phosphate tailings, that is, they have an influence on the reaction rate of phosphate tailings with acetic acid. The following single factor analysis test further analyzes and explains the influence of the above factors on the reactivity of phosphate tailings.

[0062] 1.2 Effect of calcination temperature on the reactivity of phosphate tailings

[0063] Since there are many factors affecting the calcination of phosphate tailings, in order to explore the optimal process conditions for the calcination and activation of phosphate tailings, it is necessary to further study the effect of calcination temperature on the reactivity of phosphate tailings. The specific research method is to set the calcination temperature to 750, 800, 850, and 900 ° C, and the calcination time is 10, 20, 30, 40, 50, 60, 70, 80, and 90 minutes when the heating rate is 10 ° C / min, and investigate the change of the weight loss rate of phosphate tailings, CaO and MgO activity with calcination time at different calcination temperatures.

[0064] When the weight loss rate curve of phosphate tailings is flat and unchanged, the thermal decomposition of phosphate tailings is basically completed. Therefore, the decomposition of CaMg(CO3)2 in phosphate tailings can be investigated by changing the weight loss rate curve. The change trend of weight loss rate of phosphate tailings with calcination time at different calcination temperatures is shown in the figure. Figure 3 shown.

[0065] Depend on Figure 3 It can be seen that at the selected temperature, the weight loss rate of phosphorus tailings increases with the increase of calcination time. Since the decomposition of phosphorus tailings is an endothermic decomposition process, as the calcination time increases, the more heat the phosphorus tailings absorb, the more thoroughly the phosphorus tailings decompose, and the higher the weight loss rate of phosphorus tailings. Although the weight loss rate of phosphorus tailings at different temperatures increases with the increase of calcination time, the time for the reaction to reach a complete decomposition state at different calcination temperatures is different. It can be seen that when the calcination temperature is 900℃ and 850℃, the thermal decomposition reaction has basically reached equilibrium when the reaction time is 20min; when the calcination temperature is 800℃, the thermal decomposition reaction of phosphorus tailings reaches equilibrium at 70min; when the calcination temperature is 750℃, the reaction does not reach equilibrium at 90min. This is because as the temperature increases, the diffusion rate of the reactants accelerates and the decomposition rate increases. Taking into account the reaction rate, time and economic cost, the best weight loss conditions for phosphate tailings are a calcination temperature of 800-900°C and a calcination time of 20-50 min; among them, a calcination temperature of 850°C and a calcination time of 30 min are currently the best weight loss conditions for phosphate tailings.

[0066] Figure 4 and Figure 5 This is the curve of the change of the activity of CaO and MgO in phosphate tailings with calcination time at different calcination temperatures. It can be seen from the figure that during the calcination of phosphate tailings, the activity of CaO and MgO increases with the increase of temperature, but the upward trend gradually slows down. This is because the increase in temperature activates the lattice of CaO and MgO, and the lattice volume expands due to the intensification of thermal vibration, stretching the interatomic bond length. However, as the temperature continues to rise, the crystals of CaO and MgO gradually develop completely, the crystals gradually stabilize, and the activity tends to be flat or even decreases. Therefore, considering the economic cost and the activity of CaO and MgO, it is not advisable to choose a too high calcination temperature.

[0067] At different calcination temperatures, the activity of CaO and MgO in the initial stage of the reaction increases with the increase of calcination time. This is because the lattice in the product absorbs a lot of heat and becomes active as the reaction time increases in the early stage of the reaction. When the reaction reaches a certain time, the activity of calcium oxide and magnesium oxide reaches the highest. Thereafter, as the reaction time increases, the activity of CaO and MgO tends to decrease, because too long a reaction time will cause the phosphorus tailings to overburn and lose some of their activity. When the calcination temperature is 850℃ and 900℃ and the calcination time is 30min, the activity of CaO and MgO can reach a high level.

[0068] By studying the changing trends of the weight loss rate of phosphate tailings and the activities of CaO and MgO with calcination time at different temperatures, and comprehensively considering the time and economic cost, the current optimal calcination temperature is 850℃ and the calcination time is 30min. Under this condition, the weight loss rate of phosphate tailings is 35.94%, the activity of CaO is 9.17ml, and the activity of MgO is 44.75%.

[0069] 1.3 Effect of heating rate on the reactivity of phosphate tailings

[0070] Since the muffle furnace used in the calcination of phosphorus tailings is operated according to the procedure of first heating up, then maintaining a constant temperature, and then cooling down, the muffle furnace first reaches the set temperature within a certain period of time according to the set heating rate, then maintains a certain calcination time at the set temperature, and finally cools down at a certain cooling rate. Therefore, different heating rates will affect the time required for the heating stage, and then affect the weight loss rate of phosphorus tailings, CaO and MgO activity. The experiment explores the changing trends of the weight loss rate of phosphorus tailings, CaO and MgO activity at reaction times of 10, 20, 30, 40, 50, 60, 70, 80, and 90 minutes when the calcination temperature is 850°C and the heating rates are 5, 10, 15, and 20°C / min.

[0071] The variation trend of weight loss rate of phosphate tailings with calcination time at different heating rates is as follows Figure 6 As shown. Figure 6It can be seen that when the calcination temperature is 850℃ and the heating rate is 5, 10, 15, and 20℃ / min, the weight loss rate of the phosphorus tailings shows a trend of first rising and then flattening with the increase of reaction time, and with the increase of the heating rate, the time for the weight loss rate to reach equilibrium becomes later. Under the condition of a heating rate of 5℃ / min, the weight loss rate of the phosphorus tailings remains unchanged after calcination for 20min, and the thermal decomposition is basically completed. Under the condition of a heating rate of 10, 15, and 20℃ / min, the weight loss rate of the phosphorus tailings remains unchanged after calcination for 30min, and the thermal decomposition is basically completed. This is because under the same calcination temperature, with the increase of the heating rate, the time required for the heating stage decreases. In addition, during the heating process of calcination, the phosphorus tailings have begun to absorb heat for decomposition. The reduction of the heating time will reduce the heat absorbed by the phosphorus tailings during the heating stage, thereby increasing the time to reach reaction equilibrium during the formal calcination process.

[0072] Figure 7 and Figure 8 This is the curve of the activity of CaO and MgO in phosphate tailings with calcination time at different heating rates. It can be seen from the figure that in the early stage of calcination, the activity of CaO shows a downward trend with the increase of heating rate, and the activity of CaO at different heating rates in the later stage of calcination is not much different. Within 20 minutes of calcination time, the activity of MgO decreases with the increase of heating rate. In the later stage of calcination, the activity of MgO tends to be stable at different heating rates, but the activity of MgO is the highest when the heating rate is 20℃ / min. In the early stage of calcination, the activity of CaO and MgO increases with the increase of calcination time. After the calcination time reaches 30 minutes, the activity of CaO and MgO does not change much and gradually tends to be flat. The increase in heating rate will lead to a decrease in the heating time in the early stage of heating, and the heat absorbed by the phosphate tailings will be reduced. Therefore, in the early stage of calcination, the decomposition of the phosphate tailings is not thorough enough, and the content of CaO and MgO produced by decomposition is insufficient, and the overall activity is low. In the later stage of calcination, due to the high heating rate, the material has a large temperature difference in a short period of time, and the lattice development has defects, and the activity is also higher.

[0073] Therefore, through the above research on the changing trends of the weight loss rate of phosphorus tailings and the activity of CaO and MgO with calcination time under different calcination temperatures and heating rates, and taking into account the time and economic cost, the experimental conditions for calcining and activating phosphorus tailings can be: the calcination temperature can be 800-900℃, preferably 850-900℃; the calcination time can be 20-50min, preferably 20-35min; the heating rate can be 5-20℃ / min, preferably 10-20℃ / min. Among them, the optimal experimental conditions for calcining and activating phosphorus tailings are calcination temperature of 850℃, heating rate of 20℃ / min, and calcination time of 30min. Under the optimal calcination conditions, the weight loss rate of phosphorus tailings is 35.85%, the activity of CaO is 9.33ml, and the activity of MgO is 49.74%. The particle size range of calcined phosphorus tailings is between 5.355-44.626μm, and the average particle size is 10.679μm.

[0074] Under the optimal high temperature calcination conditions, CaMg(CO3)2 in the phosphate tailings is basically completely decomposed into MgO and CaO with high activity, while Ca5(PO4)3F therein does not react. Therefore, the calcined activated phosphate tailings are mainly composed of MgO, CaO, and Ca5(PO4)3F, and its main chemical components include CaO 54.35%, MgO 23.56%, P2O5 12.86%, SiO25.36%, etc.

[0075] 2. Acetic Acid Hydrolysis

[0076] Add acetic acid solution to the round bottom jacketed reaction bottle and place it in a low temperature constant temperature tank. When the temperature of the acetic acid solution reaches the set temperature, add the calcined activated phosphate tailings formed under the optimal high temperature calcination conditions, and perform acid hydrolysis reaction at a certain stirring rate. Filter immediately after the reaction to obtain acid hydrolysis solution II and acid hydrolysis residue II.

[0077] Since the main purpose of the acetic acid hydrolysis step is to leach calcium and magnesium elements in the calcined activated phosphate tailings through acetic acid, the comprehensive utilization of the phosphate tailings and the reduction of the production cost of CMA are achieved. In order to achieve this goal, it is necessary to control the parameters such as the amount of glacial acetic acid, the liquid-to-solid ratio of the acetic acid solution and the calcined activated phosphate tailings, the reaction temperature, the reaction time, and the stirring speed.

[0078] 2.1 Effect of glacial acetic acid dosage on the leaching rate of CaO and MgO

[0079] Therefore, it is necessary to consider the cost of acetic acid and reduce the amount of acetic acid as much as possible while ensuring the calcium and magnesium leaching rate. At the same time, in order to ensure the quality of CMA obtained after subsequent evaporation and crystallization of the filtrate, it is practical to investigate and determine the amount of glacial acetic acid.

[0080] The specific research method is: according to the contents of CaO, MgO and Ca5(PO4)3F in calcined phosphate tailings, the amount of glacial acetic acid required for the complete reaction of a certain mass of calcined phosphate tailings is calculated, and the amount of acetic acid is set to 83.56%, 89.04%, 94.52%, 100.00% and 105.48% of the theoretical amount, the liquid-solid ratio is 10:1, the reaction temperature is 25°C, the stirring speed is 400r / min, and the reaction time is 30min. The effect of acetic acid dosage on the leaching rate of calcium and magnesium in calcined phosphate tailings is investigated.

[0081] The amount of glacial acetic acid consumed for the complete reaction of a certain mass of calcined phosphate tailings is calculated based on the contents of CaO, MgO and Ca5(PO4)3F in the calcined phosphate tailings. The activity of the phosphate tailings is improved after calcination, and the amount of acetic acid in the experiment can be designed within a small range around the theoretical amount. Fig. 9 The change trend of calcium and magnesium leaching rate in calcined phosphate tailings when the amount of acetic acid is 83.56%, 89.04%, 94.52%, 100.00% and 105.48% of the theoretical amount respectively under the conditions of liquid-solid ratio of 10:1, reaction temperature of 25℃, stirring rate of 400r / min and reaction time of 30min. Fig. 9 It can be seen that as the amount of acetic acid increases, the acidolysis reaction becomes more thorough, and the leaching rates of CaO and MgO also increase. When the amount of acetic acid reaches 94.52% of the theoretical amount, the reaction basically reaches equilibrium. Therefore, as the amount of acetic acid increases, the growth trend of the leaching rates of CaO and MgO becomes very gentle. Considering the leaching rates of calcium and magnesium and the cost of acetic acid, the amount of acetic acid can be selected as 89%-106% of the theoretical amount, and the optimal amount of acetic acid is 94.52% of the theoretical amount.

[0082] 2.2 Effect of liquid-to-solid ratio of acetic acid solution and calcined activated phosphate tailings on the leaching rate of CaO and MgO

[0083] Since the liquid-to-solid ratio of acetic acid solution and calcined activated phosphate tailings affects the processing volume and cost, further research is needed on the effect of the liquid-to-solid ratio of acetic acid solution and calcined activated phosphate tailings on the leaching rates of CaO and MgO.

[0084] The specific research method is: keep the optimal acetic acid dosage unchanged, set the liquid-solid ratio to 6:1, 8:1, 10:1, 12:1, and 14:1, the reaction temperature to 25°C, the stirring speed to 400r / min, and the reaction time to 30min, and investigate the effect of the liquid-solid ratio on the leaching rate of calcium and magnesium in calcined phosphate tailings.

[0085] Under the conditions of acetic acid dosage of 94.52% of the theoretical dosage, reaction temperature of 25℃, stirring speed of 400r / min and reaction time of 30min, the change trend of calcium and magnesium leaching rate in calcined phosphate tailings was investigated when the liquid-solid ratio was 6:1, 8:1, 10:1, 12:1 and 14:1 respectively. The results are shown in Fig.10 ,Depend on Fig.10 It can be seen that with the increase of liquid-to-solid ratio, the leaching rate of calcium and magnesium generally shows an upward trend. When the liquid-to-solid ratio increases to 10:1, the growth trend of CaO and MgO leaching rates slows down. As the liquid-to-solid ratio increases, the water content in the solution increases. + The diffusion capacity of ions is enhanced, and the Ca generated by the reaction 2+ Mg 2+ It can also migrate from the reaction interface to the solution in time, accelerating the reaction rate. However, when the liquid-solid ratio increases to a certain extent, further increasing the liquid-solid ratio will cause H + A too low concentration will reduce the reaction activity, and a too high liquid-to-solid ratio will also increase the cost of subsequent filtrate evaporation and crystallization. Therefore, the liquid-to-solid ratio of the acetic acid solution and the calcined activated phosphate tailings can be (6-14):1; considering the comprehensive economic benefits and reaction activity, the liquid-to-solid ratio is preferably (10-12):1, and the optimal liquid-to-solid ratio is 10:1.

[0086] 2.3 Effect of reaction time on the leaching rate of CaO and MgO

[0087] Since reaction time affects the processing volume and cost, further research is needed on the effect of reaction time on the leaching rate of CaO and MgO.

[0088] The specific research method is: keep the optimal acetic acid dosage and liquid-solid ratio unchanged, set the reaction time to 15, 20, 25, 30, 35, and 40 min, the stirring rate to 400 r / min, the reaction temperature to 25 °C, and examine the effect of reaction time on the leaching rate of calcium and magnesium in calcined phosphate tailings.

[0089] Under the conditions of acetic acid dosage of 94.52% of the theoretical dosage, liquid-solid ratio of 10:1, reaction temperature of 25°C, and stirring speed of 400r / min, the change trend of calcium and magnesium leaching rate in calcined phosphate tailings was investigated when the reaction time was 15, 20, 25, 30, 35, and 40min. The experimental results are shown in Fig.11 .Depend on Fig.11It can be seen that within the first 30 minutes of the reaction, the leaching rates of CaO and MgO in the calcined phosphate tailings increase with the increase of reaction time, and the growth trend of the leaching rate tends to be flat after 30 minutes. Because the concentration of reactants in the solution is high in the early stage, the reaction speed is fast, and the reaction is basically completed after 30 minutes of reaction, and the growth trend of the leaching rate becomes flat thereafter. Therefore, the reaction time of acetic acid hydrolysis can be 15-40 minutes; considering the calcium and magnesium leaching rates and time cost, the reaction time is preferably 25-35 minutes; and the optimal reaction time is 30 minutes.

[0090] 2.4 Acid slag analysis

[0091] (1) XRD analysis: The composition of the acid-decomposed slag II obtained by calcining the phosphate tailings with acetic acid was analyzed by X-ray diffraction. Fig.12 From the XRD diagram, it can be seen that the acid hydrolysis slag II is mainly composed of Ca5(PO4)3F (fluoroapatite) and SiO2 (quartz), which shows that CaO and MgO in the calcined phosphate tailings are basically fully involved in the reaction. The improved process conditions have greatly improved the reaction rate and degree of the reaction between phosphate tailings and acetic acid.

[0092] (2) Quantitative analysis of P2O5: The P2O5 content in the acid hydrolysis slag II increased from 12.86% before the reaction to 31.88%. It can be seen that the phosphate tailings, which were originally solid waste with a very low phosphorus content, were upgraded to high-grade phosphate ore through acetic acid hydrolysis and calcination to activate the phosphate tailings. While producing the target product, calcium magnesium acetate deicing agent, the enrichment of P2O5 in the phosphate tailings was completed, which not only solved the accumulation hazard of solid waste phosphate tailings, but also made good use of waste, alleviating the shortage of phosphate resources in my country.

[0093] (3) SEM analysis: Fig.13 This is the SEM image of acidolysis slag II obtained by acetic acid acidolysis and calcination of phosphate tailings after the reaction. The particle size of the acidolysis slag after the reaction does not change significantly, because the large particles of phosphate tailings have disintegrated and broken into small particles during the activation calcination, so the acidolysis and calcination of phosphate tailings does not change its particle size significantly.

[0094] (4) Particle size distribution analysis: The particle size of the acid hydrolysis residue II was measured using a laser particle size analyzer. The measurement conditions were: anhydrous ethanol as the dispersion medium, ultrasound for 60 seconds, and a stirring rate of 40 r / min. The measurement results are shown in Figure 2. Fig.14 It can be seen that the particle size range of the acid slag is between 3.142-41.622μm, and the average particle size is 10.157μm; the particle size range of the calcined activated phosphate tailings obtained under the aforementioned optimal calcination process conditions is between 3.142-41.622μm, and the average particle size is 10.157μm; therefore, the particle size distribution of the acid slag II and the calcined activated phosphate tailings is not much different.

[0095] Therefore, the optimal process conditions of the acetic acid hydrolysis step are: acetic acid dosage is 94.52% of the theoretical dosage, liquid-solid ratio is 10:1, reaction time is 30min, reaction temperature is 25°C, and stirring speed is 400r / min. Under the optimal process conditions of acetic acid hydrolysis, the leaching rate of CaO can reach 94.24%, the leaching rate of MgO can reach 95.53%, and the P2O5 content of the obtained acid hydrolysis slag II is increased from 12.86% before the reaction to 31.88%, which can be used as high-grade phosphate ore, thereby realizing the upgrading of low-grade phosphate tailings to high-grade phosphate ore.

[0096] 3. Evaporation Crystallization

[0097] The main purpose of this step is to purify the acid hydrolysis solution and obtain CMA crystals. Specifically, the acid hydrolysis solution formed under the optimal process conditions of acetic acid hydrolysis is placed in a rotary evaporator and evaporated and crystallized at 60°C by vacuum distillation. When the solution is evaporated to a white viscous state, it is dried in an oven at 70°C for 3 hours to obtain the following: Fig.15 The homemade Type II CMA snow melting agent shown is a white solid powder.

[0098] Among them, under the optimal process conditions of acetic acid hydrolysis, the amount of acetic acid used is not excessive, and after testing, the acid hydrolysis solution formed under the optimal process conditions of acetic acid hydrolysis does not contain acetic acid. Therefore, in this embodiment, this step can be directly carried out by evaporation crystallization without pH adjustment.

[0099] 3.1 CMA Characterization

[0100] Samples: the above-mentioned homemade type II CMA, type I CMA, and a commercially available CMA de-icing agent. Among them, the preparation method of type I CMA refers to the paper "Li Mengyu, Tang Jianwei, Liu Yong, et al. Study on the process of preparing calcium magnesium acetate de-icing agent by acetic acid hydrolysis of phosphate tailings [J]. Inorganic Salt Industry, 2024, 56(01): 73-80", that is, compared with the preparation method of type II de-icing agent, type I CMA is not subjected to high-temperature calcination treatment, but directly subjected to acetic acid hydrolysis treatment under non-calcination conditions. The acetic acid hydrolysis process parameters are: acetic acid dosage is 130% of the theoretical dosage, liquid-solid ratio is 14:1, reaction time is 3h, reaction temperature is 90℃, and stirring speed is 1000r / min; the purification crystallization process is to first add an appropriate amount of CaO to the acid hydrolysis solution to neutralize the excess acetic acid, and then perform evaporation crystallization treatment; the other steps and process parameters remain the same as those of type II CMA.

[0101] (1) Macroscopic morphology analysis. The photo of Type II CMA de-icing agent is shown in the figure below. Fig.15It is a white solid particle, and its whiteness is 90.34% as measured by an intelligent whiteness tester. The whiteness is 94.71%, which is higher than that of Type I CMA de-icing agent. The product appearance of Type II CMA de-icing agent meets the requirements of GB / T 2351-2017 that the de-icing agent must be in the form of granules or flakes.

[0102] (2) XRD analysis: The composition of each sample was analyzed by X-ray diffraction. The XRD results are shown in Fig.16 .from Fig.16 It can be seen that type II CMA is mainly composed of magnesium acetate tetrahydrate and calcium acetate hemihydrate; type II CMA is mainly composed of magnesium acetate, calcium acetate hemihydrate, and calcium acetate hydrate; the main components of a commercially available CMA de-icing agent are magnesium acetate tetrahydrate and calcium acetate hemihydrate. Therefore, the type II CMA de-icing agent prepared in the embodiment of the present invention contains the effective ingredients of calcium acetate and magnesium acetate.

[0103] (3) XRF analysis: The XRF results of Type II CMA de-icing agent and a commercially available CMA de-icing agent were analyzed and compared. The XRF results are shown in Table 2. Calcium acetate and magnesium acetate in the de-icing agent are expressed in the form of CaO and MgO. Table 2 shows that the CaO content in Type II de-icing agent is 73.97%, the MgO content is 24.91%, and the other components are 1.12%; the CaO content in a commercially available CMA de-icing agent is 29.96%, the MgO content is 69.89%, and the other components are 0.15%. According to literature research, when the molar ratio of calcium acetate and magnesium acetate in the CMA de-icing agent is 3:7, calcium and magnesium acetate reach the lowest eutectic point (-34 to -37°C), with high heat capacity and good de-icing ability. Therefore, when commercial CMA de-icing agent is made, the ratio of calcium acetate to magnesium acetate is controlled at 3:7 to achieve the best de-icing effect. Since the Ca content in the phosphate tailings raw materials is higher than that in the Mg element, the proportion of calcium acetate and magnesium acetate in the prepared CMA de-icing agent is relatively high.

[0104] Table 2 Main chemical components of two CMA deicing agents

[0105]

[0106] (4) SEM analysis: The SEM image of the homemade type II CMA is shown in Fig.17 As shown. The homemade II type CMA de-icing agent has a rod-shaped and granular structure, and the particles are dispersed and unconnected. Under high magnification, it can be seen that the surface of the particles presents a thin and long stick-shaped crystal layer. The red box area in the SEM image was scanned separately, and the EDS energy spectrum analysis of the elements contained in the area was performed. The EDS analysis results are shown in Table 3, and the mapping diagram is shown in Fig.18As shown. The green fluorescent part in the figure is calcium, and the red fluorescent part is magnesium. The calcium element accounts for a large proportion in the scanning area selected by the type II snow melting agent. From Table 3, it can be seen that the elements contained in the selected area of ​​the type II CMA snow melting agent are Ca and Mg, with atomic percentages of 67.74% and 32.26% respectively, and mass percentages of 77.58% and 22.42%.

[0107] Table 3 EDS element distribution results of type II CMA

[0108]

[0109] (5) Infrared analysis

[0110] The three CMA de-icing agents were analyzed by Fourier transform infrared spectrometer. Fig.19 As shown in the figure, it can be seen that in the infrared spectrum of the homemade type II CMA de-icing agent, 3013cm -1 1602cm is H2O stretching vibration; -1 The COO antisymmetric stretching vibration of calcium acetate is at 1532 cm -1 The position is the variable angle vibration of H2O; 1446cm -1 The asymmetric vibration of CH3 is at 1416cm-1; the symmetric stretching vibration of COO of calcium acetate is at 1346cm-1; -1 1052cm is the symmetrical angle vibration of CH3; -1 and 1027cm -1 CH3 swing vibration; 660cm -1 、643cm -1 and 617cm -1 The characteristic spectral band of calcium acetate is shown in the infrared analysis chart. The homemade type II CMA de-icing agent contains the necessary functional groups of calcium magnesium acetate de-icing agent.

[0111] In the infrared spectrum of a commercially available CMA de-icing agent, 3522 cm -1 、3095cm -1 1604cm is the stretching vibration of crystalline H2O; -1 The COO antisymmetric stretching vibration of calcium acetate is at 1531 cm -1 The angular vibration of crystalline H2O is at 1446 cm -1 The asymmetric vibration of CH3 is at 1418cm -1 The COO symmetric stretching vibration of calcium acetate is at 1350cm -1 1058cm is the symmetrical angle vibration of CH3; -1 and 1030cm -1 The CH3 rocking vibration is at 660cm -1 、643cm-1 and 624cm -1 The infrared analysis shows that a commercially available CMA de-icing agent has the necessary functional groups of calcium magnesium acetate de-icing agent.

[0112] In the infrared spectrum of type I CMA deicing agent, 3014 cm -1 1599cm is the stretching vibration of crystalline H2O; -1 The COO antisymmetric stretching vibration of calcium acetate is at 1564cm -1 The angular vibration of crystalline H2O is at 1443 cm -1 The asymmetric vibration of CH3 is at 1409cm -1 The COO symmetric stretching vibration of calcium acetate is at 1344 cm -1 1052cm is the symmetrical angle vibration of CH3; -1 and 1027cm -1 The CH3 rocking vibration is at 660cm -1 、644cm -1 and 617cm -1 The infrared analysis shows that the homemade type I CMA de-icing agent contains the necessary functional groups of calcium magnesium acetate de-icing agent.

[0113] In summary, the type II CMA provided in the embodiments of the present invention is expected to be used in the preparation of snow-melting agents.

[0114] 3.2CMA snow melting performance test

[0115] The following tests were conducted on the snow melting performance of the self-made Type II CMA, a commercially available CMA snow melting agent, Type I CMA snow melting agent and sodium chloride provided in the embodiments of the present invention. The results are shown in Tables 4-5 and Fig. 20 shown.

[0116] Table 4 Snow melting performance test results

[0117]

[0118] Table 5 Heavy metal content of different de-icing agents

[0119] sample Mercury mg / kg Cadmium mg / kg Chromium mg / kg Lead mg / kg Arsenic mg / kg Homemade Type II CMA 0.12 0.12 4.57 0.26 0.38 A commercially available CMA de-icing agent 0.0175 0.0242 1.0574 0.5722 0.3477 Type I deicing agent 0.63 0.74 2.01 0.80 1.69 International Standards ≤1 5 15 25 5

[0120] From Table 4-5 we can see that:

[0121] 1) In terms of solid dissolution rate, compared with the performance of a commercially available CMA de-icing agent and a type I CMA de-icing agent, the solid dissolution rate of type II CMA is greater than 6.0 g / min, meeting the national standard requirements. The solid dissolution rate of the type I CMA de-icing agent is superior to that of the homemade type II CMA de-icing agent in the embodiment of the present invention. This is mainly because acetic acid as an activator can promote the dissolution rate of the de-icing agent, thereby improving its efficiency in the de-icing process.

[0122] 2) In terms of pH value, the pH values ​​of various de-icing agents are similar and weakly alkaline, and all meet the requirement of GB / T 23851-2017 that the pH value of de-icing agents should be between 6.0 and 10.0.

[0123] 3) In terms of carbon steel corrosion rate, the corrosion rates of different deicing agents were tested by the coupon corrosion test method. The carbon steel corrosion rate of the self-made Type II CMA deicing agent of the embodiment of the present invention meets the national standard requirements and is lower than the carbon steel corrosion rate of the Type I CMA deicing agent. This is mainly because excessive acetic acid may increase the corrosion of the deicing agent to the metal surface, especially the corrosion rate of metals such as carbon steel. In addition, the carbon steel corrosion rate of the self-made Type II CMA deicing agent of the embodiment of the present invention is not only much lower than the carbon steel corrosion rate of sodium chloride (0.4312mm / a), but also lower than the corrosion rate of distilled water to carbon steel (0.1302mm / a).

[0124] 4) In terms of the relative damage rate of plant seeds, the relative damage rate of plant seeds of the homemade Type II CMA de-icing agent according to the embodiment of the present invention is only 9%, which is not much different from the performance of the Type I CMA de-icing agent and a certain CMA de-icing agent sold on the market, and meets the requirement of <50% stipulated in the national standard. Compared with the relative damage rate of plant seeds of sodium chloride (46%), the relative damage rate of plant seeds of the CMA de-icing agent is reduced by nearly 40%.

[0125] 5) In terms of chloride content, the self-made Type II CMA de-icing agent, Type I CMA de-icing agent, and a commercially available CMA de-icing agent as non-chloride de-icing agents meet the national standard requirement of <1.0%. Compared with chloride-type de-icing agents, CMA de-icing agents have extremely low chloride content, which is less harmful and corrosive to the environment; compared with Type I CMA de-icing agents, the self-made Type II CMA de-icing agent in the embodiment of the present invention has a lower chloride content, which is mainly because the calcined activated de-icing agent is subjected to high-temperature calcination during its preparation. During the high-temperature calcination process, some components in the raw materials, especially some volatile or unstable substances, such as chlorides, are usually effectively removed or reduced in content during the calcination process.

[0126] 6) In terms of heavy metal content, the content of heavy metals such as mercury (Hg), cadmium (Cd), chromium (Cr), lead (Pb), and arsenic (As) in two homemade CMA de-icing agents and a commercially available CMA de-icing agent was detected by inductively coupled plasma emission spectrometry. The heavy metal contents in the homemade Type II CMA de-icing agent, Type I CMA de-icing agent, and a commercially available de-icing agent in the embodiment of the present invention are all lower than the national standard requirements; however, compared with the Type I CMA de-icing agent, the homemade Type II CMA de-icing agent has relatively low Hg and As contents, and significantly higher Cr contents, mainly because high-temperature calcination can effectively remove or reduce some highly volatile heavy metals such as mercury (Hg) and arsenic (As) during the preparation process, and during the calcination process, some fixed heavy metal elements such as chromium (Cr) may be more stably retained in the product, resulting in a relatively high content in the final product. However, these chromium forms are usually relatively stable and insoluble, meeting the requirements of national standards, and will not have a significant impact on the environment and safety of use.

[0127] from Fig. 20 It can be seen from the deicing ability curve that the homemade Type II CMA in the embodiment of the present invention has a deicing ability that is basically equivalent to that of sodium chloride, and is almost the same as the deicing effect of a commercially available CMA deicing agent. After 30 minutes, the amount of ice melted by the homemade CMA is always above 90% of the amount of ice melted by NaCl, which also meets the requirements of the national standard for deicing agents. Compared with the Type I CMA deicing agent, the deicing effect of the homemade Type II CMA in the embodiment of the present invention is almost the same.

[0128] Therefore, the preparation method of type II CMA provided in the embodiment of the present invention mainly improves the activity of phosphate tailings through calcination activation of phosphate tailings, thereby improving the leaching rate of CaO and MgO, and their leaching rate exceeds 90%; the acetic acid acidolysis reaction time does not exceed 1h, and no additional heating is required during the acidolysis reaction, and the reaction can be directly carried out at room temperature; the amount of acetic acid used is greatly reduced, and can even be less than its theoretical amount, so that there is no need to adjust the pH value during the subsequent purification process, and the acidolysis solution can be directly evaporated and crystallized; the P2O5 content of the acidolysis residue can be increased to more than 30%, meeting the requirements of high-grade phosphate ore, and can be used as a direct raw material for the production of high-added phosphorus chemical products. Therefore, the method provided in the embodiment of the present invention has the characteristics of fast reaction rate, short reaction time, low economic cost, high P2O5 grade in the by-product, simplified preparation process of snow melting agent, and high economic added value of recycling of phosphate tailings.

[0129] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, ordinary technicians in the field should understand that the specific implementation methods of the present invention can still be modified or some technical features can be replaced by equivalents without departing from the spirit of the technical solution of the present invention, which should be included in the scope of the technical solution for protection of the present invention.

Claims

1. A method for preparing calcium magnesium acetate using phosphate tailings, comprising the steps of: High-temperature calcination: First, the phosphorus tailings are subjected to high-temperature calcination treatment to obtain calcined activated phosphorus tailings; Acetic acid acidolysis: uniformly mixing the acetic acid solution and the calcined activated phosphate tailings to carry out leaching reaction, filtering, and obtaining an acidolysis solution and an acidolysis residue; Purification and crystallization: subjecting the acid hydrolyzate to evaporation and crystallization treatment, and drying to obtain calcium magnesium acetate; Preferably, the phosphate tailings are dolomite-rich phosphate tailings, the main phase composition of which includes CaMg(CO3)2, Ca5(PO4)3F and SiO2, and the main elements contained include Ca, Mg, P, Si, Al, F and C; Preferably, the particle size of the phosphate tailings is 40-240 μm; the particle size of the calcined activated phosphate tailings is 5-45 μm; and the particle size of the acid-lysis slag is 3-45 μm.

2. The method according to claim 1, characterized in that The high-temperature calcination step comprises: heating the phosphate tailings to 800-900 °C at a heating rate of 5-20 °C / min and calcining for 20-50 min to obtain the calcined activated phosphate tailings, and the phase composition of the calcined activated phosphate tailings mainly includes CaO, MgO, Ca5(PO4)3F and SiO2; Preferably, the calcination temperature is 850-900 °C, the calcination time is 20-35 min, and the heating rate is 10-20 °C / min.

3. The method according to claim 1 or 2, characterized in that: The P2O5 content in the phosphate tailings does not exceed 15%; Preferably, the main chemical components of the phosphate tailings include CaO, MgO, CO2, P2O5, and SiO2.

4. The method according to claim 1 or 2, characterized in that The acetic acid hydrolysis step comprises: reacting the acetic acid solution and the calcined activated phosphate tailings at room temperature for 15-40 min under stirring, filtering, and obtaining the acid hydrolysis solution and acid hydrolysis slag, wherein the main chemical components of the acid hydrolysis solution include calcium acetate and magnesium acetate; the main phase components of the acid hydrolysis slag are Ca5(PO4)3F and SiO2; Preferably, the acetic acid hydrolysis reaction time is 25-35 min.

5. The method according to claim 4, characterized in that The amount of acetic acid in the acetic acid solution is 89%-106% of the theoretical amount of acetic acid.

6. The method according to claim 4, characterized in that The liquid-to-solid ratio of the acetic acid solution to the calcined activated phosphate tailings is (6-14): 1; Preferably, the liquid-to-solid ratio of the acetic acid solution to the calcined activated phosphate tailings is (10-12):

1.

7. The method according to claim 6, characterized in that The stirring speed is 350-450 r / min.

8. The method according to claim 1 or 6, characterized in that The room temperature is 15-35°C; Preferably, the room temperature is 20-30°C.

9. Calcium magnesium acetate prepared by the method according to any one of claims 1 to 8, characterized in that: It is mainly composed of magnesium acetate tetrahydrate and calcium acetate hemihydrate.

10. Use of the calcium magnesium acetate according to claim 9 in preparing a snow-melting agent.

Citation Information

Cited By

  • Method for preparing calcium magnesium acetate environment-friendly snow-melting corrosion inhibitor by comprehensive utilization of chlor-alkali salt mud solid waste

    CN120717883A

  • Method for preparing calcium-magnesium acetate environment-friendly snow-melting corrosion inhibitor from chlor-alkali salt mud solid waste

    CN120717883B