Method for preparing aromatic methylamine

By mixing aromatic carboxylic acid, ammonia and carrier gas, the gas solid phase catalytic reaction is carried out, and the supported catalyst is used to directly generate aromatic methylamine at a specific temperature and pressure, the problem of low preparation efficiency of aromatic amine in the prior art is solved. Achieve efficient aromatic methylamine production.

CN119039149AActive Publication Date: 2024-11-29SHANDONG GENGCAI NEW MATERIALS TECHNOLOGY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411544968.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-01
Publication Date
2024-11-29
Estimated Expiration
2044-11-01

AI Technical Summary

Technical Problem

The existing preparation methods of aromatic amines have problems such as low production efficiency and raw material conversion efficiency and complicated steps. A method of directly preparing aromatic methylamine can be required to continuously react to improve production efficiency and raw material conversion rate.

Method used

By mixing aromatic carboxylic acid, ammonia and carrier gas, preheating to the gas state, gas solid phase catalytic reaction is carried out, and aromatic methylamine is directly generated under conditions of 380~560℃, 0.05~0.25MPa, and the reaction is controlled by using a supported catalyst to directly generate aromatic methylamine at 380~560℃, 0.05~0.25MPa. Temperature and pressure to shorten the survival time of transition intermediate products and improve reaction efficiency.

Benefits of technology

The continuous reaction of directly preparing aromatic methylamine from aromatic carboxylic acid is achieved, which improves production efficiency and raw material conversion rate and simplifies the reaction control steps.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039149A_ABST
    Figure CN119039149A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of chemical engineering, and discloses a method for preparing aromatic methylamine, which comprises the following steps: 1, mixing aromatic carboxylic acid, ammonia gas and carrier gas, and preheating to a gaseous state to obtain mixed gas; and 2, carrying out a gas-solid phase catalytic reaction on the mixed gas under the conditions that the reaction temperature is 380-560 DEG C and the reaction pressure is 0.05-0.25 MPa to obtain aromatic methylamine. In the preparation process of the aromatic methylamine, the aromatic carboxylic acid is subjected to gas-phase reaction, so that continuous preparation of the aromatic methylamine can be realized, and the production efficiency is improved. By controlling the reaction temperature and pressure range, the aromatic methylamine can be directly prepared from the aromatic carboxylic acid, and the reaction control steps are reduced. By selecting the catalyst doped with multiple elements, the synergistic effect can be exerted, the duration of a transition-state intermediate product is shortened, and rapid conversion from aromatic carboxylic acid to aromatic methylamine is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention generally relates to the field of chemical technology. More specifically, the present invention relates to a method for preparing aromatic methylamine. Background Art

[0002] Aromatic amine compounds are important organic raw materials and are widely used in the production of dyes, medicines, agricultural chemicals, additives, surfactants, textile auxiliaries, chelating agents, polymers, flame retardants, etc.

[0003] The preparation of aromatic amines includes direct preparation from aromatic hydrocarbons, preparation from hydrogenation of nitrated aromatic hydrocarbons, preparation from hydrogenation of aromatic amides, etc. Most aromatic amines are prepared by reduction of aromatic nitro compounds. There are many methods for reducing nitro groups to amino groups. The methods currently used in industry to reduce nitro groups are mainly the following: metal reduction in acidic, neutral, and alkaline systems; chemical reduction; catalytic hydrogenation reduction; electrochemical reduction, etc. The catalytic hydrogenation reduction method uses precious metals such as Pd, Pt, Ni, and their alloys as catalysts to reduce nitro groups to amino groups at a certain temperature and pressure.

[0004] The preparation of aromatic amines in the prior art has problems such as low production efficiency and raw material conversion efficiency and complicated steps. There is still a need for a method that can directly prepare aromatic amines by continuous reaction to improve production efficiency and raw material conversion rate. Summary of the invention

[0005] In order to at least solve one or more of the technical problems mentioned above, the present invention provides a method for preparing aromatic methylamine, comprising: a first step of mixing an aromatic carboxylic acid, ammonia and a carrier gas, and preheating them to a gaseous state to obtain a mixed gas; a second step of subjecting the mixed gas to a gas-solid phase catalytic reaction at a reaction temperature of 380-560° C. and a reaction pressure of 0.05-0.25 MPa to obtain aromatic methylamine.

[0006] According to one embodiment of the present invention, in the mixed gas, ammonia is in excess relative to the aromatic carboxylic acid.

[0007] According to one embodiment of the present invention, in the mixed gas, the molar ratio of the aromatic carboxylic acid to the ammonia is 1:15 to 1:30.

[0008] According to one embodiment of the present invention, in the mixed gas, the molar ratio of the aromatic carboxylic acid to the ammonia is 1:20.

[0009] According to one embodiment of the present invention, in the mixed gas, ammonia accounts for 10-100% of the total volume of ammonia and carrier gas.

[0010] According to one embodiment of the present invention, in the mixed gas, ammonia accounts for 20-60% of the total volume of ammonia and carrier gas.

[0011] According to one embodiment of the present invention, the aromatic carboxylic acid is selected from: (2+4n) H (2n+4-m) (COOH) m , where n is selected from 1, 2 or 3; when n=1, m=1, 2 or 3; when n=2, m=1 or 2; when n=3, m=1.

[0012] According to one embodiment of the present invention, the aromatic carboxylic acid is selected from the group consisting of benzoic acid, isophthalic acid, terephthalic acid, 1,8-naphthalene dicarboxylic acid, 1-naphthalene dicarboxylic acid, 2-naphthalene dicarboxylic acid, 9-anthracene dicarboxylic acid, 3-phenanthracene dicarboxylic acid, 1-anthracene dicarboxylic acid, 2-anthracene dicarboxylic acid, 1,3-naphthalene dicarboxylic acid, 1,7-naphthalene dicarboxylic acid, 2-phenanthracene dicarboxylic acid, and any one of trimellitic acid.

[0013] According to one embodiment of the present invention, the carrier gas is selected from at least one of nitrogen, carbon dioxide, helium, argon, hydrogen and ammonia. Preferably, the carrier gas is selected from at least one of hydrogen and ammonia. More preferably, the carrier gas is selected from ammonia.

[0014] According to one embodiment of the present invention, the preheating temperature of the mixed gas is 200° C. to 500° C. Preferably, the preheating temperature of the mixed gas is 300° C. or 350° C.

[0015] According to one embodiment of the present invention, the reaction temperature of the gas-solid phase catalytic reaction is 400-500° C., the reaction pressure is 0.07-0.10 MPa, and the reaction time is 10-60 s.

[0016] According to one embodiment of the present invention, the catalyst for the gas-solid phase catalytic reaction is a supported catalyst, wherein the active components of the supported catalyst are selected from at least three elements of transition metals, alkali metals, alkaline earth metals, and precious metals. Preferably, the active components of the supported catalyst are selected from at least three elements of Au, P, Ti, Mo, Ru, Ni, Pt, Pd, Rh, Ag, and Co. More preferably, the active components of the supported catalyst include at least Au and Ag.

[0017] According to one embodiment of the present invention, the mass percentage of the active component to the supported catalyst is 1-10%.

[0018] According to one embodiment of the present invention, the mass percentage of the active component to the supported catalyst is 5-8%.

[0019] According to one embodiment of the present invention, the carrier of the supported catalyst is selected from SiO2, Al2O3, and TiO2.

[0020] According to one embodiment of the present invention, the carrier of the supported catalyst is Al2O3.

[0021] According to one embodiment of the present invention, the active components of the supported catalyst include the following elements: Ag: 1 part by weight; P: 0~0.5 part by weight; Ti: 0~0.3 part by weight; Mo: 0~0.3 part by weight; Ru: 0~0.4 part by weight; Ni: 0~0.5 part by weight; Pt: 0~0.2 part by weight; Pd: 0~0.3 part by weight; Rh: 0~0.3 part by weight; Au: 0~0.5 part by weight; Co: 0~0.3 part by weight.

[0022] In the preparation process of aromatic methylamine of the present invention, aromatic carboxylic acid is used as the starting point, and a gas phase reaction is carried out in the presence of ammonia and a catalyst to directly and continuously generate aromatic methylamine and by-products. In the present invention, the aromatic carboxylic acid in a gaseous state is formed by preheating, and a mixed gas is formed with ammonia and a carrier gas, so that a continuous gas phase reaction can be achieved, thereby improving production efficiency. By controlling the reaction temperature and pressure range, aromatic methylamine can be directly prepared from aromatic carboxylic acid, reducing the reaction control steps. By selecting the reaction temperature and pressure, transition state intermediate products such as aromatic amides are quickly converted into aromatic methylamines after a short duration. By selecting a catalyst doped with multiple elements, its synergistic effect can be brought into play, the duration of the transition state intermediate product is shortened, thereby improving the reaction efficiency and realizing the rapid conversion from aromatic carboxylic acid to aromatic methylamine. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] By reading the following detailed description with reference to the accompanying drawings, the above and other objects, features and advantages of the exemplary embodiments of the present invention will become readily understood. In the accompanying drawings, several embodiments of the present invention are shown in an exemplary and non-limiting manner, and the same or corresponding reference numerals represent the same or corresponding parts, wherein:

[0024] Figure 1 A schematic diagram showing the steps of a method for preparing aromatic methylamines is shown;

[0025] Figure 2 A block diagram of a reaction system suitable for use in an embodiment of the present invention is shown. DETAILED DESCRIPTION

[0026] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention.

[0027] It should be understood that the terms "include" and "comprising" used in the description and claims of the present invention indicate the presence of described features, integers, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or combinations thereof.

[0028] It should also be understood that the terms used in this specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. As used in the specification of the present invention and the claims, the singular forms of "a", "an" and "the" are intended to include the plural forms unless the context clearly indicates otherwise. It should also be further understood that the term "and / or" used in the specification of the present invention and the claims refers to any combination of one or more of the associated listed items and all possible combinations, and includes these combinations.

[0029] The specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0030] Figure 1 A schematic diagram of the steps of a method for preparing aromatic methylamines is shown.

[0031] like Figure 1 As shown, the present invention provides a method for preparing aromatic methylamine, comprising: a first step S1, mixing aromatic carboxylic acid, ammonia and a carrier gas, and preheating them to a gaseous state to obtain a mixed gas; a second step S2, subjecting the mixed gas to a gas-solid phase catalytic reaction at a reaction temperature of 380-560° C. and a reaction pressure of 0.05-0.25 MPa to obtain aromatic methylamine.

[0032] In the preparation process of the aromatic methylamine of the present invention, the aromatic carboxylic acid is used as the starting point, and a gas phase reaction is carried out in the presence of ammonia and a catalyst. The reaction can be carried out continuously to directly generate the aromatic methylamine and by-products.

[0033] The reactor applicable to the present invention includes at least one of a fixed bed, a fluidized bed, and an ebullating bed, preferably a fluidized bed or a fixed bed. The reactor is preloaded with a solid phase catalyst, and the aromatic carboxylic acid is preheated to a gaseous state and transported to the reactor together with ammonia by a carrier gas for a gas-solid phase catalytic reaction.

[0034] In the present invention, a gaseous aromatic carboxylic acid is formed by preheating, and a mixed gas is formed with ammonia and a carrier gas, so that a continuous gas phase reaction can be achieved, thereby improving production efficiency. By controlling the reaction temperature and pressure range, aromatic methylamine can be directly prepared from aromatic carboxylic acid, reducing the reaction control steps and improving the reaction efficiency.

[0035] In an embodiment of the present invention, the aromatic carboxylic acid is selected from: (2+4n) H (2n+4-m)(COOH) m , where n is selected from 1, 2 or 3; when n=1, m=1, 2 or 3; when n=2, m=1 or 2; when n=3, m=1.

[0036] Preferably, the aromatic carboxylic acid is selected from the group consisting of benzoic acid, isophthalic acid, terephthalic acid, 1,8-naphthalene dicarboxylic acid, 1-naphthalene dicarboxylic acid, 2-naphthalene dicarboxylic acid, 9-anthracene dicarboxylic acid, 3-phenanthracene dicarboxylic acid, 1-anthracene dicarboxylic acid, 2-anthracene dicarboxylic acid, 1,3-naphthalene dicarboxylic acid, 1,7-naphthalene dicarboxylic acid, 2-phenanthracene dicarboxylic acid, and trimellitic acid.

[0037] In the present invention, by preferably using the aromatic carboxylic acids shown in the above expression and the aromatic carboxylic acids listed above, rapid preheating and gasification can be achieved, with lower temperature requirements and stronger fluidity, which is suitable for large-flow production in industrial scenarios.

[0038] According to one embodiment of the present invention, the carrier gas is selected from at least one of nitrogen, carbon dioxide, helium, argon, hydrogen and ammonia. Preferably, the carrier gas is selected from at least one of hydrogen and ammonia. More preferably, the carrier gas is selected from ammonia.

[0039] In the present invention, the carrier gas may be nitrogen, carbon dioxide, helium, or argon, which are relatively inert to the hydrogenation reaction, or hydrogen and / or ammonia, which have a promoting effect on the hydrogenation reaction. When ammonia is selected as the carrier gas, ammonia can appropriately release hydrogen at the temperature and pressure specified in the present invention, thereby promoting the forward progress of the catalytic hydrogenation reaction.

[0040] According to one embodiment of the present invention, in the mixed gas, ammonia is in excess relative to the aromatic carboxylic acid. That is, the molar amount of ammonia is greater than the molar amount of the aromatic carboxylic acid. Excess ammonia can promote the catalytic hydrogenation reaction of the aromatic carboxylic acid and improve the conversion rate of the aromatic carboxylic acid. Preferably, in the mixed gas, the molar ratio of the aromatic carboxylic acid to ammonia is 1:15~1:30. More preferably, the molar ratio of the aromatic carboxylic acid to ammonia is 1:20. The molar amount of ammonia is 15 to 30 times that of the aromatic carboxylic acid. On the one hand, the conversion rate of the aromatic carboxylic acid can be improved. On the other hand, the excess ammonia can provide hydrogen during the reaction to promote the catalytic hydrogenation reaction.

[0041] According to one embodiment of the present invention, in the mixed gas, ammonia accounts for 10 to 100% of the total volume of ammonia and carrier gas. Preferably, ammonia accounts for 20 to 60% of the total volume of ammonia and carrier gas. The total volume of ammonia and carrier gas is the sum of the volume of ammonia and the volume of carrier gas. When the carrier gas is other gases other than ammonia, ammonia accounts for at least 10% to ensure that the concentration of ammonia is not lower than the reaction concentration between it and aromatic carboxylic acid. When the carrier gas is ammonia, ammonia accounts for 100%. Preferably, when the carrier gas is not ammonia, ammonia accounts for 20 to 60% of the total volume of ammonia and carrier gas, so that the concentration of ammonia is optimal, and ammonia that reacts with aromatic carboxylic acid and ammonia that provides hydrogen can be provided simultaneously.

[0042] According to one embodiment of the present invention, the preheating temperature of the mixed gas is 200°C to 500°C. Preferably, the preheating temperature of the mixed gas is 300°C or 350°C. In the present invention, the selection of the minimum preheating temperature is set differently depending on the type of aromatic carboxylic acid. The maximum preheating temperature can be set to be slightly lower than the reaction temperature of the gas-solid phase catalytic reaction, which can reduce the premature decomposition of the aromatic carboxylic acid during the process of gasifying the aromatic carboxylic acid.

[0043] According to one embodiment of the present invention, the reaction temperature of the gas-solid phase catalytic reaction is 400-500°C, the reaction pressure is 0.07-0.10 MPa, and the reaction time is 10-60 s. The reaction time is adjusted according to different reaction temperatures and reaction pressures and the catalytic capacity of the catalyst. Under the above reaction temperature, reaction pressure and other conditions, aromatic carboxylic acid and ammonia form aromatic amide or its transition intermediate product, which is hydrogenated to form aromatic methylamine under the catalytic action of the gas-solid phase catalyst. Due to the selection of the above reaction temperature and pressure, the aromatic amide or other transition intermediate product is directly converted into aromatic methylamine after a short existence.

[0044] According to one embodiment of the present invention, the catalyst for the gas-solid phase catalytic reaction is a supported catalyst, wherein the active components of the supported catalyst are selected from at least three elements of transition metals, alkali metals, alkaline earth metals, and precious metals. Preferably, the active components of the supported catalyst are selected from at least three elements of Au (gold), P (phosphorus), Ti (titanium), Mo (molybdenum), Ru (ruthenium), Ni (nickel), Pt (platinum), Pd (palladium), Rh (rhodium), Ag (silver), and Co (cobalt). More preferably, the active components of the supported catalyst include at least Au (gold) and Ag (silver).

[0045] Transition metals mainly refer to all elements of groups IIIB, IVB, VB, VIB, VIIB, as well as groups VIII, IB, and IIB.

[0046] Precious metals mainly refer to gold, silver and platinum group metals (ruthenium, rhodium, palladium, osmium, iridium and platinum).

[0047] Alkaline earth metals mainly refer to beryllium, magnesium, calcium, strontium, barium and radium.

[0048] Alkali metals mainly refer to lithium, sodium, potassium, rubidium, cesium and francium.

[0049] The active component can be randomly selected from the above metals. Preferably, the active component must contain Ag and / or Au.

[0050] In the present invention, by selecting catalysts doped with multiple elements, their synergistic effect can be exerted to shorten the lifetime of the transition intermediate of aromatic methylamine, so that it can be quickly converted into aromatic methylamine, thereby improving the reaction efficiency and realizing the rapid conversion from aromatic carboxylic acid to aromatic methylamine.

[0051] The catalytic hydrogenation reaction is not only related to the adsorption and dissociation of hydrogen, but also closely related to the adsorption of substrate molecules and the desorption of product molecules. By selecting at least three of the above catalysts, the hydrogenation activity of a single-type atomic catalyst can be broken through, thereby achieving an efficient hydrogenation reaction. According to the inventor's research, Au (gold) and Ag (silver) have a strong synergistic effect with the above other catalysts, so the preferred active component is a mixture of gold and silver with other catalysts. In addition, the sharing of the above multiple catalysts plays an important role in improving the stability of the catalyst.

[0052] In the present invention, the absolute amount of the catalyst can be adjusted according to parameters such as the amount of the aromatic carboxylic acid, ammonia and other reactants in the reactor, the size of the reactor and the like.

[0053] According to one embodiment of the present invention, the carrier of the supported catalyst is selected from SiO2, Al2O3, and TiO2. Preferably, the carrier is Al2O3. The above carrier can provide multiple pore sizes, large specific surface area, and high dispersibility.

[0054] According to one embodiment of the present invention, the mass percentage of the active component to the supported catalyst is 1-10%. For example, it can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, etc., preferably 5-8%. The above ratio can provide a larger specific surface area for the catalytic hydrogenation reaction.

[0055] According to one embodiment of the present invention, the active components of the supported catalyst include the following elements: Ag: 1 part by weight; P: 0~0.5 part by weight; Ti: 0~0.3 part by weight; Mo: 0~0.3 part by weight; Ru: 0~0.4 part by weight; Ni: 0~0.5 part by weight; Pt: 0~0.2 part by weight; Pd: 0~0.3 part by weight; Rh: 0~0.3 part by weight; Au: 0~0.5 part by weight; Co: 0~0.3 part by weight.

[0056] For example, the formula is Ag: 1 part by weight; P: 0.5 part by weight; Ti: 0.3 part by weight; Mo: 0.3 part by weight; Ru: 0.4 part by weight; Ni: 0.5 part by weight; Pt: 0.2 part by weight; Pd: 0.3 part by weight; Rh: 0.3 part by weight; Au: 0.5 part by weight; Co: 0.3 part by weight, or based on the above formula, reduce one or more of the other components except silver.

[0057] Preferably, the active component is composed of Ag-P-Ni-Pt-Rh in a weight ratio of 1:0.40:0.30:0.09:0.15.

[0058] Preferably, the active component is composed of Ag-Ni-Pt-Au-P-Rh in a weight ratio of 1:0.30:0.09:0.10:0.40:0.15.

[0059] Preferably, the active component is composed of Ag-Ni-Pt-Mo-Ti-Ru in a weight ratio of 1:0.30:0.09:0.15:0.10:0.25.

[0060] Preferably, the active component is composed of Ag-Ni-Pt-Au-Mo-Ru in a weight ratio of 1:0.30:0.09:0.10:0.05:0.25.

[0061] Preferably, the active component is composed of Ag-Ni-Pt-Au-Co in a weight ratio of 1:0.30:0.09:0.40:0.20.

[0062] Preferably, the active component is composed of Ag-Ni-Pt-Au-P-Rh-Ru-Mo in a weight ratio of 1:0.30:0.09:0.40:0.40:0.15:0.25:0.05.

[0063] Preferably, the active component is composed of Ag-Ni-Pt-Au-P-Rh-Ru in a weight ratio of 1:0.30:0.09:0.40:0.40:0.15:0.25.

[0064] Preferably, the active component is composed of Ag-P-Ni-Pt-Rh-Mo in a weight ratio of 1:0.40:0.30:0.09:0.15:0.05.

[0065] Preferably, the active component is composed of Ag-P-Ni-Pt-Rh in a weight ratio of 1:0.10:0.30:0.09:0.15.

[0066] Preferably, the active component is composed of Ag-Au-Mo-Ni-Pt-Ru in a weight ratio of 1:0.10:0.05:0.30:0.09:0.25.

[0067] In this formula, silver is used as the main catalyst and other components are used as auxiliary catalysts. When the amount of other elements other than silver is 0, pure silver is used as the catalyst. In the present invention, it is preferred that at least two other elements other than silver are included as auxiliary catalysts. By setting the above weight ratio, the catalytic activity of silver on the catalytic hydrogenation reaction of aromatic carboxylic acids can be improved.

[0068] By preloading the above-mentioned supported gas-solid phase catalyst in the reactor, the catalytic hydrogenation reaction of aromatic carboxylic acid can be carried out continuously.

[0069] Figure 2 A block diagram of a reaction system suitable for use in an embodiment of the present invention is shown.

[0070] like Figure 2 As shown, aromatic carboxylic acid, ammonia and carrier gas are input into mixer 1 for mixing and preheating. When mixing and preheating are completed, the preheated mixed gas is input into reactor 2 from mixer 1. The temperature and pressure are controlled in reactor 2. The mixed gas is subjected to gas-phase continuous reaction under the catalysis of the supported gas-solid catalyst preinstalled in reactor 2. The obtained products include aromatic methylamine and by-products such as amides and nitriles. The products are collected in collector 3.

[0071] The following examples are provided to illustrate the reaction process of the present invention.

[0072] Example 1.

[0073] A supported catalyst whose active components consist of Ag-P-Ni-Pt-Rh in a weight ratio of 1:0.40:0.30:0.09:0.15 and whose carrier is Al2O3 is loaded in a fluidized bed.

[0074] Benzoic acid, ammonia and nitrogen are mixed in a mixer at a molar ratio of 1:15:40, and heated to 200°C during the mixing process to obtain a mixed gas. The mixed gas is introduced into a fluidized bed from the mixer, and the reaction temperature is controlled to be 420°C, the reaction pressure is controlled to be 0.08MPa, and the residence time of the mixed gas in the fluidized bed is 30s. The product in the fluidized bed is collected in a collector for detection.

[0075] After testing, the product contained benzylamine, benzonitrile and a small amount of benzamide, among which the conversion rate of benzoic acid was 99.8%, and the molar yield of benzylamine reached 50.1%.

[0076] Example 2.

[0077] Based on Example 1, the molar ratio of benzoic acid, ammonia and nitrogen was adjusted to 1:20:40, the reaction temperature was controlled to 560°C, the reaction pressure was 0.25 MPa, and the residence time of the mixed gas in the fluidized bed was 28 seconds. The product in the fluidized bed was collected in a trap for detection.

[0078] After testing, the product contained benzylamine, benzonitrile and a small amount of benzamide, among which the conversion rate of benzoic acid was 99.9% and the molar yield of benzylamine reached 56.3%.

[0079] Example 3.

[0080] Based on Example 1, the molar ratio of benzoic acid, ammonia and nitrogen was adjusted to 1:15:12.5, the reaction temperature was controlled to 380°C, the reaction pressure was 0.05 MPa, and the residence time of the mixed gas in the fluidized bed was 60 seconds. The product in the fluidized bed was collected in a trap for detection.

[0081] After testing, the product contains benzylamine, benzonitrile and a small amount of benzamide, among which the conversion rate of benzoic acid is 99.9% and the molar yield of benzylamine reaches 39.2%.

[0082] Example 4.

[0083] A supported catalyst whose active components consist of Ag-P-Ni-Pt-Rh in a weight ratio of 1:0.40:0.30:0.09:0.15 and whose carrier is Al2O3 is loaded in a fluidized bed.

[0084] Benzoic acid and ammonia are mixed in a mixer at a molar ratio of 1:160, and heated to 200°C during the mixing process to obtain a mixed gas. The mixed gas is introduced into a fluidized bed from the mixer, and the reaction temperature is controlled to be 560°C, the reaction pressure is controlled to be 0.25MPa, and the residence time of the mixed gas in the fluidized bed is 10s. The product in the fluidized bed is collected in a collector for detection.

[0085] After testing, the product contains benzylamine, benzonitrile and a small amount of benzamide, among which the conversion rate of benzoic acid is 99.8%, and the molar yield of benzylamine reaches 54.9%. It can be seen that the conversion rate and yield are both high when ammonia is used as the carrier gas.

[0086] Example 5.

[0087] A supported catalyst whose active components consist of Ag-P-Ni-Pt-Rh in a weight ratio of 1:0.40:0.30:0.09:0.15 and whose carrier is Al2O3 is loaded in a fluidized bed.

[0088] Benzoic acid, ammonia and hydrogen are mixed in a mixer at a molar ratio of 1:100:40, and heated to 200°C during the mixing process to obtain a mixed gas. The mixed gas is introduced into a fluidized bed from the mixer, and the reaction temperature is controlled to be 420°C, the reaction pressure is controlled to be 0.10 MPa, and the residence time of the mixed gas in the fluidized bed is 10 seconds. The product in the fluidized bed is collected in a collector for detection.

[0089] After testing, the product contains benzylamine, benzonitrile and a small amount of benzamide, among which the conversion rate of benzoic acid is 99.8%, and the molar yield of benzylamine reaches 57.6%. It can be seen that when hydrogen is used as the carrier gas, the conversion rate of benzoic acid and the molar yield of benzylamine are both high.

[0090] Example 6.

[0091] A supported catalyst whose active components consist of Ag-P-Ni-Pt-Rh in a weight ratio of 1:0.40:0.30:0.09:0.15 and whose carrier is Al2O3 is loaded in a fluidized bed.

[0092] Benzoic acid, ammonia and nitrogen are mixed in a mixer at a molar ratio of 1:15:135, and heated to 200°C during the mixing process to obtain a mixed gas. The mixed gas is introduced into a fluidized bed from the mixer, and the reaction temperature is controlled to be 420°C, the reaction pressure is controlled to be 0.08MPa, and the residence time of the mixed gas in the fluidized bed is 10s. The product in the fluidized bed is collected in a collector for detection.

[0093] After testing, the product contains benzylamine, benzonitrile and benzamide, among which the conversion rate of benzoic acid is 79.1%, and the molar yield of benzylamine reaches 13.7%.

[0094] Example 7.

[0095] A supported catalyst whose active components consist of Ag-Ni-Pt-Au-P-Rh in a weight ratio of 1:0.30:0.09:0.10:0.40:0.15 and whose carrier is Al2O3 is loaded in a fluidized bed.

[0096] Benzoic acid, ammonia and nitrogen are mixed in a mixer at a molar ratio of 1:20:40, and heated to 200°C during the mixing process to obtain a mixed gas. The mixed gas is introduced into a fluidized bed from the mixer, and the reaction temperature is controlled to be 380°C, the reaction pressure is controlled to be 0.08MPa, and the residence time of the mixed gas in the fluidized bed is 27.5s. The product in the fluidized bed is collected in a collector for detection.

[0097] After testing, the product contained benzylamine, benzonitrile and a small amount of benzamide, among which the conversion rate of benzoic acid was 99.2%, and the molar yield of benzylamine reached 42.1%.

[0098] Example 8.

[0099] On the basis of Example 7, the reaction temperature was adjusted from 380°C to 560°C at intervals of 20°C, and the products were tested to obtain benzoic acid conversion rates and molar yields of benzylamine at different reaction temperatures as shown in Table 1.

[0100] Table 1

[0101] Serial number Reaction temperature / ℃ Benzoic acid conversion rate / % Benzylamine molar yield / % 1 400 99.6 47.8 2 420 99.8 50.4 3 440 99.8 51.3 4 460 99.0 44.5 5 480 98.7 41.2 6 500 98.2 40.4 7 540 98.4 34.6 8 560 98.1 30.8

[0102] Example 9.

[0103] On the basis of Example 7, the reaction temperature was set to 420° C., the reaction pressure was adjusted to 0.07 and 0.10 MPa, and the products were detected to obtain the benzoic acid conversion rate and the molar yield of benzylamine under different reaction pressures as shown in Table 2.

[0104] Table 2

[0105] Serial number Reaction temperature / ℃ Reaction pressure / MPa Benzoic acid conversion rate / % Benzylamine molar yield / % 1 420 0.07 99.5 49.2 2 420 0.10 99.8 49.9

[0106] Example 10.

[0107] On the basis of Example 7, different active components of the supported catalyst were replaced, and the reaction temperature was set to 420° C. The products were tested to obtain the benzoic acid conversion rate and the molar yield of benzylamine in the presence of different supported catalysts, as shown in Table 3.

[0108] Table 3

[0109] Serial number Supported catalyst active components Benzoic acid conversion rate / % Benzylamine molar yield / % 1 Ag-Ni-Pt-Mo-Ti-Ru1:0.30:0.09:0.15:0.10:0.25 99.7 50.0 2 Ag-Ni-Pt-Au-Mo-Ru1:0.30:0.09:0.10:0.05:0.25 99.2 48.9 3 Ag-Ni-Pt-Au-Co1:0.30:0.09:0.40:0.20 99.8 49.3 4 Ag-Ni-Pt-Au-P-Rh-Ru-Mo1:0.30:0.09:0.40:0.40:0.15:0.25:0.05 99.9 51.7 5 Ag-Ni-Pt-Au-P-Rh-Ru1:0.30:0.09:0.40:0.40:0.15:0.25 99.8 51.5

[0110] Example 11.

[0111] The active components loaded in the fluidized bed are composed of Ag-P-Ni-Pt-Rh in a weight ratio of 1:0.40:0.30:0.09:0.15, and the carrier is a loaded catalyst of TiO2.

[0112] 1,3-Benzenedicarboxylic acid, ammonia and nitrogen were mixed in a mixer at a molar ratio of 1:15:40, and heated to 350°C during the mixing process to obtain a mixed gas. The mixed gas was introduced into a fluidized bed from the mixer, and the reaction temperature was controlled to be 460°C, the reaction pressure was controlled to be 0.08MPa, and the residence time of the mixed gas in the fluidized bed was 30s. The product in the fluidized bed was collected in a collector for detection.

[0113] After testing, the product contained 1,3-phenylenediamine, isophthalonitrile and a small amount of 3-cyanobenzamide, among which the conversion rate of 1,3-phthalic acid was 99.6%, and the molar yield of 1,3-phenylenediamine reached 44.5%.

[0114] Example 12.

[0115] On the basis of Example 11, different active components of the supported catalyst were replaced, and the reaction temperature was set to 420° C. The products were tested to obtain the conversion rates of 1,3-phthalic acid and the molar yields of 1,3-phenylenediamine in the presence of different supported catalysts, as shown in Table 4.

[0116] Table 4

[0117] Serial number Supported catalyst active components 1,3-Phthalic acid conversion rate / % 1,3-phenylenediamine molar yield / % 1 Ag-Ni-Pt-Au-P-Rh1:0.30:0.09:0.10:0.40:0.15 99.4 45.3 2 Ag-Ni-Pt-Mo-Ti-Ru1:0.30:0.09:0.15:0.10:0.25 99.2 44.8

[0118] Example 13.

[0119] The active components loaded in the fluidized bed are composed of Ag-P-Ni-Pt-Rh in a weight ratio of 1:0.40:0.30:0.09:0.15, and the carrier is a supported catalyst of SiO2.

[0120] 1,4-phthalic acid, ammonia and nitrogen were mixed in a mixer at a molar ratio of 1:20:40, and heated to 350°C during the mixing process to obtain a mixed gas. The mixed gas was introduced into a fluidized bed from the mixer, and the reaction temperature was controlled to be 440°C, the reaction pressure was controlled to be 0.08MPa, and the residence time of the mixed gas in the fluidized bed was 30s. The product in the fluidized bed was collected in a collector for detection.

[0121] After testing, the product contains 1,4-phenylenediamine, terephthalonitrile and a small amount of 4-cyanobenzamide, among which the conversion rate of 1,4-phthalic acid is 99.8%, and the molar yield of 1,4-phenylenediamine reaches 42.3%.

[0122] Example 14.

[0123] On the basis of Example 13, different active components of the supported catalyst were replaced, and the reaction temperature was set to 420° C. The products were tested to obtain the conversion rates of 1,4-phthalic acid and the molar yields of 1,4-phenylenediamine in the presence of different supported catalysts, as shown in Table 5.

[0124] Table 5

[0125] Serial number Supported catalyst active components 1,4-phthalic acid conversion rate / % 1,4-phenylenediamine molar yield / % 1 Ag-Ni-Pt-Au-P-Rh1:0.30:0.09:0.10:0.40:0.15 99.5 43.9 2 Ag-Ni-Pt-Mo-Ti-Ru1:0.30:0.09:0.15:0.10:0.25 99.0 42.6

[0126] Example 15.

[0127] The active components loaded in the fluidized bed are composed of Ag-P-Ni-Pt-Rh-Mo in a weight ratio of 1:0.40:0.30:0.09:0.15:0.05, and the carrier is Al2O3.

[0128] 2-naphthoic acid, ammonia and nitrogen are mixed in a mixer at a molar ratio of 1:20:40, and heated to 300°C during the mixing process to obtain a mixed gas. The mixed gas is introduced from the mixer into a fluidized bed, the reaction temperature is controlled to be 480°C, the reaction pressure is controlled to be 0.01MPa, and the residence time of the mixed gas in the fluidized bed is 30s. The product in the fluidized bed is collected in a collector for detection.

[0129] After testing, the product contains 2-naphthylamine, 2-naphthylcarbonitrile and a small amount of 2-naphthylamide, among which the conversion rate of 2-naphthic acid is 98.9%, and the molar yield of 2-naphthylamine reaches 38.7%.

[0130] Example 16.

[0131] On the basis of Example 15, different active components of the supported catalyst were replaced, the reaction temperature was set to 420°C, and the reaction pressure was set to 0.08 MPa. The products were tested to obtain the conversion rates of 2-naphthoic acid and the molar yields of 2-naphthylamine in the presence of different supported catalysts, as shown in Table 6.

[0132] Table 6

[0133] Serial number Supported catalyst active components 2-Naphthoic acid conversion rate / % 2-Naphthylmethylamine molar yield / % 1 Ag-Ni-Pt-Au-P-Rh1:0.30:0.09:0.10:0.40:0.15 99.1 39.1 2 Ag-Ni-Pt-Mo-Ti-Ru1:0.30:0.09:0.15:0.10:0.25 99.1 38.0

[0134] Example 17.

[0135] The active components loaded in the fluidized bed are composed of Ag-Ni-Pt-Au-P-Rh in a weight ratio of 1:0.30:0.09:0.40:0.40:0.15, and the carrier is Al2O3.

[0136] 1,8-naphthalene dicarboxylic acid, ammonia and nitrogen were mixed in a mixer at a molar ratio of 1:20:40, and heated to 300°C during the mixing process to obtain a mixed gas. The mixed gas was introduced into a fluidized bed from the mixer, and the reaction temperature was controlled to be 420°C, the reaction pressure was controlled to be 0.08MPa, and the residence time of the mixed gas in the fluidized bed was 30s. The product in the fluidized bed was collected in a collector for detection.

[0137] After testing, the product contains 1,8-naphthalenediamine, 1,8-naphthalenedinitrile and a small amount of 1,8-naphthalenedicarbamide, among which the conversion rate of 1,8-naphthalenedicarboxylic acid is 99.4%, and the molar yield of 1,8-naphthalenediamine reaches 32.8%.

[0138] Example 18.

[0139] On the basis of Example 17, different aromatic carboxylic acids were replaced, and other conditions remained unchanged. The products were tested to obtain different aromatic carboxylic acid conversion rates and molar yields of aromatic methylamines, as shown in Table 7.

[0140] Table 7

[0141] Serial number Aromatic carboxylic acids Aromatic carboxylic acid conversion rate / % Molar yield of aromatic methylamine / % 1 1-Naphthoic acid 99.0 37.6 2 1-Anthracenecarboxylic acid 98.9 34.6 3 2-Anthracenecarboxylic acid 98.3 34.2 4 1,3-Naphthalene dicarboxylic acid 99.2 31.3

[0142] Example 19.

[0143] On the basis of Example 17, the active component of the supported catalyst was replaced with Ag-Ni-Pt-Au-P-Rh in a weight ratio of 1:0.30:0.09:0.10:0.40:0.15. Different aromatic carboxylic acids were replaced, different preheating temperatures were set, and other conditions remained unchanged. The products were tested to obtain different aromatic carboxylic acid conversion rates and molar yields of aromatic methylamines as shown in Table 8.

[0144] Table 8

[0145] Serial number Aromatic carboxylic acids Preheating temperature / ℃ Aromatic carboxylic acid conversion rate / % Molar yield of aromatic methylamine / % 1 1,7-Naphthalene dicarboxylic acid 300 99.1 30.8 2 2-Phenanthroline 400 98.7 31.3 3 Trimellitic acid 350 98.2 25.4

[0146] Example 20.

[0147] The active components loaded in the fluidized bed are composed of Ag-Au-P-Ni-Pt-Rh in a weight ratio of 1:0.10:0.40:0.30:0.09:0.15, and the carrier is Al2O3.

[0148] 1,3-Benzenedicarboxylic acid, ammonia and hydrogen were mixed in a mixer at a molar ratio of 1:20:40, and heated to 350°C during the mixing process to obtain a mixed gas. The mixed gas was introduced into a fluidized bed from the mixer, and the reaction temperature was controlled to be 420°C, the reaction pressure was controlled to be 0.10 MPa, and the residence time of the mixed gas in the fluidized bed was 30 seconds. The product in the fluidized bed was collected in a collector for detection.

[0149] After testing, the product contains 1,3-phenylenediamine, isophthalonitrile and a small amount of 3-cyanobenzamide, among which the conversion rate of 1,3-phthalic acid is 99.8%, and the molar yield of 1,3-phenylenediamine reaches 40.6%.

[0150] Example 21.

[0151] The active components loaded in the fluidized bed are composed of Ag-P-Ni-Pt-Rh in a weight ratio of 1:0.10:0.30:0.09:0.15, and the carrier is Al2O3.

[0152] 1,3-Benzenedicarboxylic acid, ammonia and argon were mixed in a mixer at a molar ratio of 1:20:40, and heated to 350°C during the mixing process to obtain a mixed gas. The mixed gas was introduced into a fluidized bed from the mixer, and the reaction temperature was controlled to be 460°C, the reaction pressure was controlled to be 0.08MPa, and the residence time of the mixed gas in the fluidized bed was 30s. The product in the fluidized bed was collected in a collector for detection.

[0153] After testing, the product contains 1,3-phenylenediamine, isophthalonitrile and a small amount of 3-cyanobenzamide, benzonitrile and benzylamine. Among them, the conversion rate of 1,3-phthalic acid is 99.2%, and the molar yield of 1,3-phenylenediamine reaches 45.7%.

[0154] Example 22.

[0155] The active components loaded in the fluidized bed are composed of Ag-Au-Mo-Ni-Pt-Ru in a weight ratio of 1:0.10:0.05:0.30:0.09:0.25, and the carrier is Al2O3.

[0156] 9-Anthracenecarboxylic acid, ammonia and nitrogen are mixed in a mixer at a molar ratio of 1:30:40, and heated to 350°C during the mixing process to obtain a mixed gas. The mixed gas is introduced into a fluidized bed from the mixer, and the reaction temperature is controlled to be 480°C, the reaction pressure is controlled to be 0.01MPa, and the residence time of the mixed gas in the fluidized bed is 30s. The product in the fluidized bed is collected in a collector for detection.

[0157] The product was tested to contain 9-anthracenemethylamine, 9-anthracenecarbonitrile and a small amount of 9-anthracenecarboxamide, wherein the conversion rate of 9-anthracenecarboxylic acid was 99.1%, and the molar yield of 9-anthracenemethylamine reached 33.9%.

[0158] Example 23.

[0159] The active components loaded in the fluidized bed are composed of Ag-Au-Mo-Ni-Pt-Ru in a weight ratio of 1:0.10:0.05:0.30:0.09:0.25, and the carrier is Al2O3.

[0160] 3-phenanthroline carboxylic acid, ammonia and nitrogen are mixed in a mixer at a molar ratio of 1:20:40, and heated to 500°C during the mixing process to obtain a mixed gas. The mixed gas is introduced into a fluidized bed from the mixer, and the reaction temperature is controlled to be 500°C, the reaction pressure is controlled to be 0.10MPa, and the residence time of the mixed gas in the fluidized bed is 30s. The product in the fluidized bed is collected in a collector for detection.

[0161] After testing, the product contained 3-phenanthrenylamine, 3-phenanthrenylcarbonitrile and a small amount of 3-phenanthrenylcarboxamide, among which the conversion rate of 3-phenanthrenylcarboxylic acid was 99.3%, and the molar yield of 3-phenanthrenylamine reached 32.6%.

[0162] Example 24.

[0163] The active components loaded in the fluidized bed are composed of Ag-Au-Mo-Ni-Pt-Ru in a weight ratio of 1:0.10:0.05:0.30:0.09:0.25, and the carrier is Al2O3.

[0164] 1,3,5-benzenetricarboxylic acid, ammonia and nitrogen were mixed in a mixer at a molar ratio of 1:30:40, and heated to 350°C during the mixing process to obtain a mixed gas. The mixed gas was introduced into a fluidized bed from the mixer, and the reaction temperature was controlled to be 460°C, the reaction pressure was controlled to be 0.10 MPa, and the residence time of the mixed gas in the fluidized bed was 30 seconds. The product in the fluidized bed was collected in a collector for detection.

[0165] After testing, the product contains 1,3,5-benzenetrimethylamine, 1,3,5-benzenetricarbonitrile, benzonitrile and a small amount of benzamide, among which the conversion rate of 1,3,5-benzenetricarboxylic acid is 98.1%, and the molar yield of 1,3,5-benzenetrimethylamine reaches 21.8%.

[0166] Although multiple embodiments of the present invention have been shown and described herein, it will be apparent to those skilled in the art that such embodiments are provided by way of example only. Those skilled in the art may conceive of many changes, modifications, and alternatives without departing from the thought and spirit of the present invention. It should be understood that in the process of practicing the present invention, various alternatives to the embodiments of the present invention described herein may be adopted. The appended claims are intended to define the scope of protection of the present invention, and therefore cover equivalents or alternatives within the scope of these claims.

Claims

1. A method for preparing aromatic methylamine, characterized in that: include: In the first step, aromatic carboxylic acid, ammonia and carrier gas are mixed and preheated to a gaseous state to obtain a mixed gas; In the second step, the mixed gas is subjected to a gas-solid phase catalytic reaction at a reaction temperature of 380-560° C. and a reaction pressure of 0.05-0.25 MPa to obtain aromatic methylamine.

2. The method according to claim 1, characterized in that: In the mixed gas, ammonia is in excess relative to the aromatic carboxylic acid, and ammonia accounts for 10-100% of the total volume of ammonia and carrier gas.

3. The method according to claim 1, characterized in that The aromatic carboxylic acid is selected from: (2+4n) H (2n+4-m) (COOH) m , wherein n is selected from 1, 2 or 3; When n=1, m=1, 2 or 3; When n=2, m=1 or 2; When n=3, m=1.

4. The method according to claim 1, characterized in that: The carrier gas is selected from at least one of nitrogen, carbon dioxide, helium, argon, hydrogen and ammonia.

5. The method according to claim 1, characterized in that: The carrier gas is selected from at least one of hydrogen and ammonia.

6. The method according to claim 1, characterized in that The catalyst for the gas-solid phase catalytic reaction is a supported catalyst, wherein the active components of the supported catalyst are selected from at least three elements of transition metals, alkali metals, alkaline earth metals, and noble metals.

7. The method according to claim 6, characterized in that The carrier of the supported catalyst is selected from any one of SiO2, Al2O3, and TiO2.

8. The method according to claim 6, characterized in that The active components of the supported catalyst are selected from at least three elements of Au, P, Ti, Mo, Ru, Ni, Pt, Pd, Rh, Ag and Co.

9. The method according to claim 8, characterized in that The active components of the supported catalyst include at least Au and Ag.

10. The method according to claim 8, characterized in that The active components of the supported catalyst include the following elements: Ag: 1 part by weight; P: 0-0.5 parts by weight; Ti: 0-0.3 parts by weight; Mo: 0-0.3 parts by weight; Ru: 0-0.4 parts by weight; Ni: 0-0.5 parts by weight; Pt: 0-0.2 parts by weight; Pd: 0-0.3 parts by weight; Rh: 0-0.3 parts by weight; Au: 0-0.5 parts by weight; Co: 0-0.3 parts by weight.

Citation Information

Patent Citations

  • Manufacturing method of nitrile and corresponding amine thereof

    CN104557357A

  • Manufacturing method for nitrile and corresponding amine thereof

    CN105001032A

  • Method for preparing 1, 6-hexamethylenediamine from 5-hydroxymethylfurfural

    CN112898164A

  • Preparation method of xylylenediamine and cyclohexanedimethylamine

    CN116444381A

  • Method for producing xylylenediamine

    JP2012082146A