Layered vanadium-oxygen hybrid material as well as preparation method and application thereof
Through the hydrothermal synthesis of layered vanadium oxy hybrid material [C4H8NH2]V3O7, the existing adsorbent materials have poor selectivity and complex process when treating radioactive wastewater of rare earth ore, and the efficient separation of uranium and europium is achieved. Recycling, with radiation resistance, acid and alkali resistance and thermal stability, suitable for radioactive wastewater treatment of rare earth ore under different pH conditions.
Patent Information
- Application Number
- CN202411155746.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-22
AI Technical Summary
The existing adsorbent materials have poor selectivity when treating radioactive wastewater from rare earth ore, narrow pH range and complex preparation technology, which cannot meet the treatment needs of radioactive wastewater from rare earth ore.
The layered vanadium oxy hybrid material [C4H8NH2]V3O7 is synthesized by hydrothermal method, which has radiation resistance, acid and alkali resistance and thermal stability, and is used to efficiently separate and recover uranium and europium in radioactive wastewater of rare earth-associated ore. Simple process and low cost.
It realizes efficient exchange and separation of uranium and europium, has good radiation resistance, acid and alkali resistance and thermal stability, and is suitable for radioactive wastewater treatment of rare earth-associated ore under different pH conditions, reducing treatment costs.
Smart Images

Figure CN119039200A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of wastewater treatment, and in particular relates to a layered vanadium-oxygen hybrid material and a preparation method and application thereof. Background Art
[0002] my country is relatively rich in mineral resources with associated radioactive elements. There are many types of ores that can be developed, such as rare earth ores, zircon ores, tantalum-niobium ores, and vanadium ores. These ores are usually accompanied by natural radioactive elements such as uranium, thorium, and radium. During the mining process, radioactive wastewater from rare earth associated ores is easily produced, posing a potential risk of radioactive pollution to my country's ecological environment.
[0003] At present, the adsorption materials used to treat radioactive wastewater are limited by problems such as poor selective adsorption performance, narrow applicable pH range and complex preparation process, and can no longer meet the treatment needs of radioactive wastewater from rare earth associated minerals. Summary of the invention
[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a layered vanadium-oxygen hybrid material and a preparation method and application thereof, which not only has a simple preparation process and low cost, but also the prepared [C4H8NH2]V3O7 has good radiation stability, acid and alkali resistance and thermal stability, and can simultaneously and efficiently separate and recover uranium and europium in rare earth associated mine radioactive wastewater.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] A layered vanadium-oxygen hybrid material with a chemical formula of [C4H8NH2]V3O7 and a space group of P21 / c.
[0007] Furthermore, the layered vanadium-oxygen hybrid material can withstand 400 kGy of γ and β particle radiation, and the decomposition temperature is higher than 350° C., and the tolerable pH value is 1.5 to 13.5.
[0008] A method for preparing a layered vanadium-oxygen hybrid material comprises the following steps:
[0009] Step 1, adding vanadium pentoxide to deionized water at a molar ratio of 1:(100-130), stirring, and obtaining an orange-yellow solution I;
[0010] Step 2, add a tetrahydropyrrole solution having a concentration of 211 mg / g to the orange-yellow solution I in a volume ratio of (40-50 mL): (1-4 mL), and stir to obtain an orange-yellow solution II;
[0011] Step 3, adjusting the pH value of the orange-yellow solution II to weak acidity, stirring, and obtaining an orange-yellow solution III;
[0012] Step 4, transfer the orange-yellow solution III into a polytetrafluoroethylene reactor liner, tighten the reactor, place it in an oven at 180-200°C, and perform hydrothermal synthesis reaction for 5 days. After the reaction is completed, filter and obtain a black solid product;
[0013] Step 5: After centrifugation and washing for several times, the black solid product is dried to obtain a layered vanadium-oxygen hybrid material [C4H8NH2]V3O7.
[0014] Furthermore, the stirring in step 1 and step 3 is carried out at a speed of 300 to 500 r / min and magnetic stirring at room temperature for 1 hour.
[0015] Furthermore, the stirring in step 2 is carried out at a speed of 300 to 500 r / min and magnetic stirring at room temperature for 5 hours.
[0016] Furthermore, in step 3, acetic acid is used to adjust the pH value of the orange-yellow solution II to 4.5-6.5.
[0017] Furthermore, the washing in step 5 is performed by centrifugation washing three times each with deionized water and anhydrous ethanol.
[0018] Furthermore, the drying in step 5 is carried out in an oven at 60 to 90° C. for 18 to 30 hours.
[0019] The application of layered vanadium-oxygen hybrid materials in the treatment of radioactive wastewater from rare earth associated mines is to adsorb uranium and europium in radioactive wastewater from rare earth associated mines.
[0020] Compared with the prior art, the present invention has the following technical effects:
[0021] Organic amine ion [THPH] in layered vanadium-oxygen hybrid material [C4H8NH2]V3O7 of the present invention + It can efficiently exchange uranium and europium, and realize the separation and recovery of uranium and europium in radioactive wastewater from rare earth associated mines. Moreover, [C4H8NH2]V3O7 has radiation stability, acid and alkali resistance, and thermal stability, which is specifically reflected in: it can withstand 400kGy of γ and β particle radiation, the decomposition temperature is not lower than 350°C, and it can stably exist under the condition of pH=1.5-13.5. It is suitable for treating radioactive wastewater from rare earth associated mines under different conditions, thereby meeting the existing treatment needs of radioactive wastewater from rare earth associated mines in my country.
[0022] The present invention adopts a hydrothermal method to adjust the inorganic open skeleton [V3O7] under the structural guidance of the organic amine tetrahydropyrrole C4H8NH n- structure, [C4H8NH2] n+ Inserted as cation into inorganic open framework [V3O7] n-The layered structure of the structure is used to obtain an open-framework layered vanadium-oxygen hybrid material [C4H8NH2]V3O7. Not only is the process simple, the cost is low, and the yield is as high as 86%, but by regulating the pH, reaction time and reaction temperature, open-framework layered vanadium-oxygen hybrid materials with different morphologies and chemical properties can be obtained to meet different application requirements.
[0023] When the [C4H8NH2]V3O7 of the present invention is used to treat radioactive wastewater from rare earth associated minerals, the organic amine ion [THPH] + It can efficiently exchange uranium and europium, and simultaneously separate and recover uranium and europium. It not only has a high ion response speed, reaching equilibrium in 15 minutes, but also has a high distribution coefficient. Among them: in real rare earth associated mine radioactive wastewater, the distribution coefficient of uranium K d U =2.90×10 3 mL / g, distribution coefficient K of europium d Eu =6.92×10 2 mL / g, and the removal rates of uranium and europium reached R U =74.37% and R Eu =40.89%; in the simulated rare earth associated mine radioactive wastewater, K d U =5.69×10 3 mL / g,K d Eu =1.27×10 3 mL / g,R U =85.04%, R Eu =55.90%; in addition, after ion exchange, 0.85mol / L KCl solution is used to elute [C4H8NH2]V3O7 adsorbed with uranium and europium to recover uranium and europium, and the layered vanadium-based crystal structure remains unchanged, so it can be used repeatedly, reducing the cost of rare earth associated mineral wastewater treatment. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The XRD pattern of the layered vanadium-oxygen hybrid material prepared in Example 1 of the present invention;
[0025] Figure 2 XRD patterns of the layered vanadium-oxygen hybrid material prepared in Example 1 of the present invention before and after irradiation;
[0026] Figure 3 XRD patterns of the layered vanadium-oxygen hybrid material prepared in Example 1 of the present invention at different pH values;
[0027] Figure 4The uranium and europium treatment capacity of the layered vanadium-oxygen hybrid material prepared in Example 1 of the present invention in simulated rare earth associated mineral wastewater;
[0028] Figure 5 The treatment capacity of the layered vanadium-oxygen hybrid material prepared in Example 2 of the present invention for uranium and europium in real rare earth associated mineral wastewater;
[0029] Figure 6 The scanning electron microscope images of the layered vanadium-based hybrid material prepared in Example 1 of the present invention before and after ion exchange;
[0030] Figure 7 This is the TG-DSC test spectrum of the layered vanadium-oxygen hybrid material prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0031] The specific contents of the present invention are further explained in detail below in conjunction with embodiments.
[0032] Example 1
[0033] Step 1, add 3.64 g of vanadium pentoxide into 40 mL of deionized water, and stir magnetically for 1 h at room temperature at a speed of 420 r / min to obtain an orange-yellow solution I;
[0034] Step 2, 1.8 mL of 211 mg / g tetrahydropyrrole solution was added dropwise to the orange-yellow solution I, and the mixture was stirred magnetically at room temperature at a speed of 420 r / min for 5 h to obtain an orange-yellow solution II;
[0035] Step 3, add acetic acid to the orange-yellow solution II, adjust the pH to 5, and stir magnetically at room temperature at a speed of 420 r / min for 1 h to obtain an orange-yellow solution III;
[0036] Step 4, transfer the orange-yellow solution III to a 100 mL polytetrafluoroethylene reactor liner, tighten the reactor, place it in an oven at 190°C, react for 5 days, and after the reaction is completed, filter to obtain a black solid product;
[0037] Step 5: Place the black solid product in a 100 mL centrifuge tube, wash it three times with deionized water and three times with anhydrous ethanol, then place it in an oven at 80° C. and dry it for 24 hours to obtain a layered vanadium-oxygen hybrid material [C4H8NH2]V3O7.
[0038] from Figure 1 It can be seen that the layered vanadium-oxygen hybrid material [C4H8NH2]V3O7 prepared by the hydrothermal method in Example 1 has high purity and high crystallinity.
[0039] from Figure 2It can be seen that after the layered vanadium-based hybrid material prepared in Example 1 was irradiated with 300 kGy and 400 kGy of γ and β particles, the intensity of the diffraction peak remained almost unchanged compared with the original sample (pristine product) that was not irradiated with γ and β particles, and the original structure was still maintained, indicating that the layered vanadium-based hybrid material prepared in Example 1 can withstand 400 kGy of γ and β particle radiation and has good radiation resistance stability required for removing radioactive nuclides.
[0040] from Figure 3 It can be seen that the intensity of the diffraction peak of the layered vanadium-oxygen hybrid material prepared in Example 1 hardly changes compared with the original sample at different pH values, indicating that it can stably exist in the pH range of 1.5 to 13.5 and has good acid and alkali stability.
[0041] At room temperature of 25°C, the layered vanadium-oxygen hybrid material prepared in Example 1 was added to simulated rare earth associated mineral wastewater at a solid-liquid ratio of 1:1000. The concentration of uranium in the simulated rare earth associated mineral wastewater was 5.95 ppm, the concentration of europium was 7.37 ppm, the concentrations of competing ions Na, Ca, Mg, Al, Fe and Mn were 24.12 ppm, 29.06 ppm, 24.40 ppm, 12.35 ppm, 17.07 ppm and 7.63 ppm, respectively, and the pH value was 6.3. The results are shown in Figure 4 Table 1;
[0042] from Figure 4 It can be seen that after ion exchange, the distribution coefficients of uranium and europium are K d U =5.69×10 3 mL / g,K d Eu =1.27×10 3 mL / g, indicating that in the presence of a large number of competing ions (including alkali metals, alkaline earth metals and transition metal ions), the layered vanadium-based hybrid material can highly selectively exchange ions with uranium and europium in simulated wastewater.
[0043] In Table 1, C0 represents the concentration of each metal ion in the simulated rare earth associated mine wastewater, C e represents the concentration of each metal ion in the simulated rare earth associated mine wastewater after ion exchange, K d represents the distribution coefficient of each metal ion after ion exchange. It can be seen from Table 1 that after ion exchange, the removal rates of uranium and europium in wastewater are R U =85.04%, R Eu =55.90%, indicating that the layered vanadium-oxygen hybrid material prepared in Example 1 has excellent adsorption performance for uranium and europium in rare earth associated mineral wastewater.
[0044] After ion exchange, the layered vanadium-based hybrid material adsorbed with uranium and europium was eluted with a KCl solution with a concentration of 0.85 mol / L. After elution, the crystal structure of the layered vanadium-based hybrid material remained unchanged, indicating that it has good stability and can be used repeatedly, reducing the cost of rare earth associated mineral wastewater treatment.
[0045] Table 1 Test data of ion exchange performance of layered vanadium-based hybrid materials in simulated rare earth associated mineral wastewater
[0046]
[0047] When the layered vanadium-oxygen hybrid material prepared in Example 1 is added to the radioactive wastewater of rare earth associated mines with a uranium concentration of 1.3 ppm, the uranium in the wastewater can be removed to below 30 ppb, meeting the national drinking water standard, further illustrating that the layered vanadium-oxygen hybrid material prepared in Example 1 has excellent adsorption performance for uranium in the radioactive wastewater of rare earth associated mines.
[0048] from Figure 6 It can be seen that, compared with before ion exchange, after ion exchange, the nanosheets in the flower-like particles of the layered vanadium-based hybrid material prepared in Example 1 became significantly thinner.
[0049] from Figure 7 It can be seen that the layered vanadium-oxygen hybrid material prepared in Example 1 begins to decompose at 350° C., indicating that it has good thermal stability.
[0050] Example 2
[0051] Step 1, add 4.55 g of vanadium pentoxide into 50 mL of deionized water, and stir the mixture with a magnetic stirrer at 420 r / min for 1 h at room temperature to obtain an orange-yellow solution I;
[0052] Step 2, add 3 mL of 211 mg / g tetrahydropyrrole solution to the orange-yellow solution I, and stir the mixture with a magnetic stirrer at room temperature and a speed of 420 r / min for 5 h to obtain an orange-yellow solution II;
[0053] Step 3, add acetic acid to the orange-yellow solution II, adjust the pH to 6, and stir magnetically at room temperature at a speed of 420 r / min for 1 h to obtain an orange-yellow solution III;
[0054] Step 4, transfer the orange-yellow solution III to a 100 mL polytetrafluoroethylene reactor liner, tighten the reactor, place it in an oven at 185°C, react for 5 days, and after the reaction is completed, filter to obtain a black solid product;
[0055] Step 5: Place the black solid product in a 100 mL centrifuge tube, wash it three times with deionized water and three times with anhydrous ethanol, then place it in an oven at 80° C. and dry it for 24 hours to obtain a layered vanadium-oxygen hybrid material [C4H8NH2]V3O7.
[0056] At room temperature of 25°C, the layered vanadium-oxygen hybrid material prepared in Example 2 was added to real rare earth associated mineral wastewater at a solid-liquid ratio of 1:1000. The concentration of uranium in the real rare earth associated mineral wastewater was 3.94 ppm, the concentration of europium was 8.51 ppm, the concentrations of competing ions Na, Ca, Mg, Al, Fe and Mn were 1.50 ppm, 14.92 ppm, 1.80 ppm, 10.06 ppm, 14.78 ppm and 2.35 ppm, respectively, and the pH value was 6.7. The results are shown in Figure 5 Table 2;
[0057] from Figure 5 It can be seen that after ion exchange, the distribution coefficients of uranium and europium are K d U =2.90×10 3 mL / g and K d Eu =6.92×10 2 mL / g, indicating that the layered vanadium-based hybrid material prepared in Example 2 can selectively undergo ion exchange with uranium and europium in real rare earth associated mineral wastewater.
[0058] In Table 2, C0 represents the concentration of each metal ion in the real rare earth associated mine wastewater, C e represents the concentration of each metal ion in the real rare earth associated mine wastewater after ion exchange, K d represents the distribution coefficient of each metal ion after ion exchange. It can be seen from Table 1 that after ion exchange, the removal rates of uranium and europium in wastewater are R U =74.37%, R Eu =40.89%, indicating that the layered vanadium-oxygen hybrid material prepared in Example 2 has excellent adsorption performance for uranium and europium in rare earth associated mineral wastewater.
[0059] After the ion exchange, the layered vanadium-based hybrid material adsorbed with uranium and europium is eluted with a KCl solution having a concentration of 0.85 mol / L, and the crystal structure of the layered vanadium-based hybrid material remains unchanged after the elution.
[0060] Table 2 Test data of ion exchange performance of layered vanadium-based hybrid materials in real rare earth associated mineral wastewater
[0061]
[0062] Example 3
[0063] Step 1, add 4 g of vanadium pentoxide to 40 mL of deionized water, and stir magnetically for 1 h at room temperature at a speed of 300 r / min to obtain an orange-yellow solution I;
[0064] Step 2, add 1 mL of 211 mg / g tetrahydropyrrole solution to the orange-yellow solution I, and stir the mixture with a magnetic stirrer at room temperature and a speed of 300 r / min for 5 h to obtain an orange-yellow solution II;
[0065] Step 3, adding acetic acid to the orange-yellow solution II, adjusting the pH to 4.5, and stirring the mixture magnetically at 300 r / min for 1 h at room temperature to obtain an orange-yellow solution III;
[0066] Step 4, transfer the orange-yellow solution III to a 100 mL polytetrafluoroethylene reactor liner, tighten the reactor, place it in an oven at 180°C, react for 5 days, and after the reaction is completed, filter to obtain a black solid product;
[0067] Step 5: Place the black solid product in a 100 mL centrifuge tube, wash it three times with deionized water and anhydrous ethanol, then place it in an oven at 60° C. and dry it for 30 hours to obtain a layered vanadium-oxygen hybrid material [C4H8NH2]V3O7.
[0068] Example 4
[0069] Step 1, add 3.78 g of vanadium pentoxide to 45 mL of deionized water, and stir magnetically for 1 h at room temperature at a speed of 500 r / min to obtain an orange-yellow solution I;
[0070] Step 2, add 2.5 mL of 211 mg / g tetrahydropyrrole solution to the orange-yellow solution I, and stir the mixture with a magnetic stirrer at room temperature and a speed of 500 r / min for 5 h to obtain an orange-yellow solution II;
[0071] Step 3, adding acetic acid to the orange-yellow solution II, adjusting the pH to 6.5, and stirring the mixture magnetically at room temperature at a speed of 500 r / min for 1 h to obtain an orange-yellow solution III;
[0072] Step 4, transfer the orange-yellow solution III to a 100 mL polytetrafluoroethylene reactor liner, tighten the reactor, place it in an oven at 195°C, react for 5 days, and after the reaction is completed, filter to obtain a black solid product;
[0073] Step 5: Place the black solid product in a 100 mL centrifuge tube, wash it three times with deionized water and three times with anhydrous ethanol, then place it in an oven at 70° C. and dry it for 20 hours to obtain a layered vanadium-oxygen hybrid material [C4H8NH2]V3O7.
[0074] Example 5
[0075] Step 1, add 3.9 g of vanadium pentoxide to 50 mL of deionized water, and stir magnetically for 1 h at room temperature at a speed of 300 r / min to obtain an orange-yellow solution I;
[0076] Step 2, 4 mL of 211 mg / g tetrahydropyrrole solution was added dropwise to the orange-yellow solution I, and the mixture was stirred magnetically at room temperature at a speed of 300 r / min for 5 h to obtain an orange-yellow solution II;
[0077] Step 3, adding acetic acid to the orange-yellow solution II, adjusting the pH to 5, and stirring the mixture magnetically at 300 r / min for 1 h at room temperature to obtain an orange-yellow solution III;
[0078] Step 4, transfer the orange-yellow solution III into a 100 mL polytetrafluoroethylene reactor liner, tighten the reactor, place it in an oven at 200° C., react for 5 days, and after the reaction is completed, filter to obtain a black solid product;
[0079] Step 5: Place the black solid product in a 100 mL centrifuge tube, wash it three times with deionized water and three times with anhydrous ethanol, then place it in an oven at 90° C. and dry it for 18 hours to obtain a layered vanadium-oxygen hybrid material [C4H8NH2]V3O7.
Claims
1. A layered vanadium-oxygen hybrid material, characterized in that: The chemical formula is [C4H8NH2]V3O7 and the space group is P21 / c.
2. The layered vanadium-based hybrid material according to claim 1, characterized in that: It can withstand 400kGy of γ and β particle radiation, and its decomposition temperature is not less than 350℃. Its tolerable pH value is 1.5 to 13.
5.
3. A method for preparing a layered vanadium-based hybrid material as claimed in claim 1 or 2, characterized in that: The steps include: Step 1, adding vanadium pentoxide to deionized water at a molar ratio of 1:(100-130), stirring, and obtaining an orange-yellow solution I; Step 2, adding a tetrahydropyrrole solution having a concentration of 211 mg / g to the orange-yellow solution I in a volume ratio of (40-50): (1-4), stirring, to obtain an orange-yellow solution II; Step 3, adjusting the pH value of the orange-yellow solution II to weak acidity, stirring, and obtaining an orange-yellow solution III; Step 4, transfer the orange-yellow solution III into a polytetrafluoroethylene reactor liner, tighten the reactor, place it in an oven at 180-200°C, and perform hydrothermal synthesis reaction for 5 days. After the reaction is completed, filter and obtain a black solid product; Step 5: After centrifugation and washing for several times, the black solid product is dried to obtain a layered vanadium-oxygen hybrid material [C4H8NH2]V3O7.
4. The method for preparing a layered vanadium-based hybrid material according to claim 3, characterized in that: The stirring in step 1 and step 3 is carried out at a speed of 300 to 500 r / min and magnetic stirring at room temperature for 1 hour.
5. The layered vanadium-based hybrid material according to claim 3, characterized in that: The stirring in step 2 is carried out at a speed of 300 to 500 r / min and magnetic stirring at room temperature for 5 hours.
6. The method for preparing a layered vanadium-based hybrid material according to claim 3, characterized in that: In step 3, acetic acid is used to adjust the pH value of the orange-yellow solution II to 4.5-6.
5.
7. The method for preparing a layered vanadium-based hybrid material according to claim 3, characterized in that: The washing in step 5 is performed by centrifugation washing three times each with deionized water and anhydrous ethanol.
8. The method for preparing a layered vanadium-based hybrid material according to claim 3, characterized in that: The drying in step 5 is performed in an oven at 60 to 90° C. for 18 to 30 hours.
9. The use of the layered vanadium-based hybrid material according to claim 1 or 2 in the treatment of radioactive wastewater from rare earth associated minerals, characterized in that: Used to adsorb uranium and europium in radioactive wastewater from rare earth associated mines.
Citation Information
Patent Citations
Uranium separation method and uranium adsorption material
CN110523396A
Inorganic-organic hybrid material based on uranium-containing wastewater treatment as well as preparation method and application of inorganic-organic hybrid material
CN116371367A
Amorphous organic hybrid vanadyl material as well as preparation method and application thereof
CN117142520A
Uranium capture on inorganic-organic graphite-based hybrid material: adsorbent material for mining reclamation and domestic water uses