Preparation method of heat-resistant high-strength high-toughness modified vinyl ester resin system

By blending the tetrafunctional compound containing diproglyglyrhezyl and diallyl groups with vinyl ester resin and adding a curing agent and accelerator, the shortcomings of traditional vinyl ester resin in terms of mechanical and heat resistance are solved. Modified resins with high heat resistance and mechanical properties are prepared, which are suitable for the production of composite materials.

CN119039530AActive Publication Date: 2024-11-29EAST CHINA UNIV OF SCI & TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411134908.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-29
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

Traditional vinyl ester resins have shortcomings in mechanical properties and heat resistance, especially in high temperature environments, and have poor processability.

Method used

A tetrafunctional compound containing diproglyglyrhezyl and diallyl groups is blended with a vinyl ester resin, and a curing agent and accelerator are added to the mixture. The modified resin is prepared by ultrasonic and mechanical stirring, and a step-curing process is adopted to Improve the thermal stability and mechanical properties of the resin.

Benefits of technology

The modified vinyl ester resin prepared has low viscosity, good stability, excellent processing performance, and high heat resistance and mechanical properties, which are suitable for the production of composite materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039530A_ABST
    Figure CN119039530A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a heat-resistant high-strength high-toughness modified vinyl ester resin system, and belongs to the technical field of thermosetting resin materials. The vinyl ester resin system is formed by mixing a four-functionality compound containing dipropargyl and diallyl as a reactive modifier with vinyl ester resin, a peroxide curing agent and an accelerant, and the vinyl ester resin system can be subjected to thermocuring to obtain a cured product of the vinyl ester resin system. The modified vinyl ester resin system prepared by the method disclosed by the invention has the advantages of high heat resistance, high strength, high toughness and the like, is suitable for manufacturing fiber reinforced composite materials by various processes such as resin transfer molding (RTM), winding molding, prepreg laying molding and the like, and is applied to the engineering technical fields of buildings, chemical industry, marine industry and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for preparing a heat-resistant high-strength and high-toughness modified vinyl ester resin system, belonging to the field of thermosetting resin materials. Background Art

[0002] Vinyl ester resin is a compound containing multiple unsaturated double bonds in its structure obtained by the reaction of unsaturated acid (such as methyl methacrylate and acrylic acid) and oligomer with active sites (such as epoxy resin) under the action of phase transfer catalyst. It is a liquid resin obtained by mixing it with styrene or methacrylate as an active diluent. It is also referred to as vinyl resin and is a recognized corrosion-resistant resin. Vinyl ester resin is a thermosetting resin that combines the chemical resistance, excellent mechanical properties, heat resistance of epoxy resin and the rapid curing characteristics of unsaturated polyester resin. It has excellent chemical resistance, thermal stability, fatigue resistance and mechanical properties. It has low viscosity and is easy to process. It has good wettability with reinforcing materials and can be cured at room temperature and heated. It is used to make fiber-reinforced composite materials and is widely used in chemical, transportation, aerospace, marine, construction, and electronic appliances. However, the current traditional vinyl ester resin has the inherent disadvantages of low strength and high brittleness, and poor high temperature resistance.

[0003] As the application fields gradually expand, especially in many anti-corrosion projects, materials are often required to be able to be used normally at higher temperatures and have higher mechanical properties, which puts higher requirements on the strength, toughness and heat resistance of the matrix resin of the composite material.

[0004] In terms of toughening vinyl ester resins, the most common methods are to add rubber as a second phase to the resin system for toughening (patent application 202011580204.9) and polyurethane toughened modified vinyl ester resin (patent application 201911206917.6). However, although the introduction of nitrile rubber segments will significantly improve the toughness of the resin, it will reduce the strength and heat resistance of the material. When polyurethane grafting is used for toughening, multifunctional isocyanates react with hydroxyl groups in the vinyl ester resin during the reaction process, the viscosity of the system increases rapidly, the reaction is difficult to control, and the risk of gelation is extremely high, which is not conducive to the processing of resin-based composite materials. Therefore, it is necessary to develop a method for toughening vinyl ester resins that can simultaneously improve heat resistance and strength and has good processability.

[0005] Propargyl terminated resin (PTR) is a high performance resin with aromatic groups in the main chain and propargyl ethers at the end. The glass transition temperature (T g) can generally exceed 300 ° C and has excellent thermal stability in air and nitrogen. In addition, PTR has the advantages of easy synthesis, relatively low cost, low moisture absorption rate, low dielectric constant and excellent adhesion, and can be used to manufacture advanced resin-based composite materials. In addition to being a single resin system, PTR is more used as a modifier to heat-resistantly modify other resin systems to form a high-performance resin system. Ge et al. (Reactive and Functional Polymers. 2023, 186: 105570.) used magnolol as a raw material to synthesize a new bio-based allyl compound with an aromatic propargyl ether group, the structure of which is shown in the following formula (a), and then used it to copolymerize with 4,4'-bismaleimide diphenylmethane (BDM) to develop a new high-performance bio-based resin. Compound (a) contains two allyl groups and two propargyl groups in the molecule, the purpose of which is to form a complex and dense cross-linked network after copolymerization with BDM to improve the mechanical properties and heat resistance of the bismaleimide resin system. Studies have shown that this blended resin has higher thermal and mechanical properties than other bio-based allyl compound modified BDM. After curing, the resin has a glass transition temperature higher than 440°C, a storage modulus greater than 1.3 GPa, a thermal decomposition temperature of about 448°C, and a flexural strength range of 106 to 117 MPa.

[0006]

[0007] The above method of modifying resin using compounds containing dipropargyl ether and diallyl is simple and effective, but the cost of using honokiol as raw material is expensive, which is not conducive to further application. The synthesis of compounds containing dipropargyl ether and diallyl tetrafunctional groups needs to reduce costs, and has not been applied to the modification of vinyl ester resins. Summary of the invention

[0008] The purpose of the present invention is to overcome the technical deficiencies of the existing vinyl ester resins, namely, the mechanical properties are not high enough and the heat resistance is not good, and at the same time, the mechanical properties and heat resistance of the vinyl ester resins are improved. The present invention provides a method for modifying the vinyl ester resin by blending a novel monomer containing a dipropargyl diallyl group as a modifier with the vinyl ester resin, and the obtained modified blended resin has the characteristics of easy preparation, good processing performance, good thermal stability, excellent mechanical properties, etc.

[0009] The present invention solves the above technical problems through the following technical solutions.

[0010] A method for preparing a heat-resistant high-strength and high-toughness modified vinyl ester resin, characterized in that the preparation method comprises the following steps:

[0011] (1) mixing a tetrafunctional compound containing a dipropargyl group and a diallyl group with a vinyl ester resin in a mass ratio of 1:1 to 1:5;

[0012] (2) simultaneously ultrasonically and mechanically stirring the mixture of step (1) at 25-30° C. to prepare a vinyl ester resin blend;

[0013] (3) adding 0.1% to 5% of the weight of the resin blend of the curing agent and 0.1% to 1% of the accelerator to the vinyl ester resin blend, stirring until homogeneous, and standing to remove bubbles;

[0014] (4) pouring the product obtained in step (3) into a mold coated with a release agent, and curing at 60 to 250° C. to obtain the modified vinyl ester resin system;

[0015] Wherein: the vinyl ester resin in step (1) is a bisphenol A epoxy vinyl ester resin or a phenolic epoxy vinyl ester resin, and its acid value is lower than 10 mgKOH / g and its room temperature viscosity is lower than 800 mPa s;

[0016] The tetrafunctional compound containing a dipropargyl group and a diallyl group in step (1) is diallyl bisphenol A dipropargyl ether, and its structural formula is shown in Formula I:

[0017] Formula I

[0018]

[0019] The curing agent used in step (3) is one or a mixture of more than one selected from methyl ethyl ketone peroxide, acetylacetone peroxide, cyclohexanone peroxide, benzoyl peroxide, dilauroyl peroxide, tert-butyl perbenzoate, dibenzoyl peroxide and tert-butyl hydroperoxide;

[0020] The promoter used in step (3) is one or a mixture of more than one selected from the group consisting of cobalt isooctanoate, cobalt cyclopentadiene cobalt, dicyclopentadiene nickel, nickel acetylacetonate, dimethylaniline and diethylaniline.

[0021] Preferably, the vinyl ester resin in step (1) is a phenolic epoxy vinyl ester resin.

[0022] Preferably, the ultrasound in step (2) is carried out in an ultrasonic water bath, with a stirring speed of 250 rpm and a stirring time of 10 to 15 min.

[0023] Preferably, the curing agent in step (3) is methyl ethyl ketone peroxide or tert-butyl perbenzoate, and the amount used is 0.5%-2% of the weight of the vinyl ester resin blend; the accelerator is cobalt isooctanoate or cobalt cyclohexaneate, and the amount used is 0.5% of the weight of the vinyl ester resin blend.

[0024] Preferably, in step (3), the temperature for adding the curing agent and the accelerator into the blended resin is 30-50° C., the stirring time is 10-20 min, and the standing time is 10-20 min.

[0025] Preferably, the stirring time in step (3) is 10 min and the standing time is 15 min.

[0026] Preferably, the curing method in step (4) is preferably step curing, which is carried out according to the following steps: keeping warm at 60-80°C for 2-4h, keeping warm at 100-200°C for 1-2h, and keeping warm at 200-250°C for 3-5h. After curing, the obtained product is naturally cooled to 25-30°C.

[0027] The tetrafunctional compound containing dipropargyl and diallyl groups shown in formula I can be prepared by a one-pot reaction. Diallyl bisphenol A is used as the main raw material and reacted with 3-halogenated-1-propyne (propargyl halide) by a phase transfer catalyst method to obtain diallyl bisphenol A dipropargyl ether. Diallyl bisphenol A and a phase transfer catalyst tetrabutylammonium bromide are added to an alkaline aqueous solution, propargyl bromide is added after stirring, and the reaction is carried out at 70-90°C for a certain time. After the oil phase is separated, it is washed with water, dried and filtered, and the solvent is removed by reduced pressure distillation to obtain diallyl bisphenol A dipropargyl ether.

[0028] The reagents and raw materials used in the present invention are commercially available.

[0029] Beneficial Effects

[0030] The positive and progressive effects of the present invention are: (1) The diallyl bisphenol A dipropargyl ether used is prepared by a one-pot method, which is simple, low-cost, and suitable for mass production. (2) The method of using diallyl bisphenol A dipropargyl ether to modify vinyl ester resin proposed in the present invention is the first to be proposed and is innovative. (3) The obtained modified vinyl ester resin has low viscosity, is stable, and has good processing performance. (4) The modified vinyl ester resin after curing has both high heat resistance and mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 is the hydrogen nuclear magnetic resonance spectrum of diallyl bisphenol A dipropargyl ether ( 1 H NMR) spectrum.

[0032] Figure 2 The differential scanning calorimetry (DSC) spectra of the vinyl ester resin blends of Examples 1-4 after adding a curing agent and an accelerator are shown.

[0033] Figure 3 The dynamic thermodynamic analysis (DMA) curves of the modified vinyl ester resin system of Example 1 and the cured resin of Comparative Example 1 are shown.

[0034] Figure 4 The thermogravimetric analysis (TGA) curves of the modified vinyl ester resin system prepared in Example 1 and the cured vinyl ester resin of Comparative Example 1 are shown.

[0035] FIG. 5( a ) and FIG. 5( b ) are scanning electron microscope (SEM) images of the impact cross-section of the modified vinyl ester resin system prepared in Example 1 and the cured vinyl ester resin of Comparative Example 1. Specific implementation methods

[0036] In order to more clearly and completely illustrate the technical solution and advantages of the present invention, the technical solution of the present invention is described in detail below through embodiments. The described embodiments are only part of the embodiments of the present invention and are only used for illustration, but not for limiting the scope of the present invention.

[0037] The diallyl bisphenol A dipropargyl ether in the example of the present invention is a tetrafunctional compound containing a dipropargyl group and a diallyl group, and its synthesis is different from the method reported in the literature (Reactive and Functional Polymers.2023,186:105570.). It is obtained by phase transfer catalysis reaction of allyl bisphenol A (DABPA) with propargyl halide in an aqueous phase system, without using a large amount of organic solvent and being environmentally friendly. The propargyl halide is propargyl bromide or propargyl chloride, and the phase transfer catalyst is tetrabutylammonium bromide or benzyltriethylammonium chloride.

[0038] In the present invention, the diallyl bisphenol A dipropargyl ether (BAPPP) is synthesized according to the above method. Specifically, 30.84g (0.1mol) of DABPA, 6.45g (0.02mol) of tetrabutylammonium bromide, 20g of NaOH (0.5mol), and 200mL of deionized water are added to a 500mL four-necked flask in sequence, and DABPA is completely dissolved at room temperature by strong mechanical stirring. 26.17g (0.22mol) of 3-bromopropyne is dissolved in toluene, and added dropwise to the system within 30min, and the reaction is carried out at 80°C constant temperature overnight. After the reaction is completed, the upper oil phase is separated, washed with alkaline water until neutral, anhydrous sodium sulfate is added to dry the organic phase, filtered and then the solvent is removed by rotary evaporation, and the residual volatiles are removed by drying at 100°C in a vacuum oven for 1h to obtain 33.72g of a dark yellow liquid product with a yield of 87.2%.

[0039] The above product BAPPP hydrogen nuclear magnetic resonance spectrometer ( 1 H NMR was performed using a Bruker AVANCE III 400 superconducting Fourier transform nuclear magnetic resonance spectrometer with an operating frequency of 400 MHz, deuterated DMSO as the solvent, and TMS as the internal standard.

[0040] The phenolic epoxy vinyl ester resin used in the examples and comparative examples of the present invention can be purchased from the market and used directly without further treatment, such as MFE 780 vinyl ester resin produced by Huachang Polymer Co., Ltd. of East China University of Science and Technology.

[0041] The carbon fiber material used in the present invention is T300 carbon fiber plain weave cloth (200g / m 2 ) and used directly without further processing.

[0042] Other reagents used in the examples of the present invention were purchased from commercially available chemically pure reagents and used directly without further treatment.

[0043] The step-wise temperature rise program of thermal curing of the modified vinyl ester resin in the examples of the present invention is determined based on the curing exothermic curve of the modified resin after blending obtained by differential scanning calorimetry (DSC), and the specific curing process is related to the mass fraction of the raw materials used in the resin.

[0044] In the following examples and comparative examples:

[0045] The curing behavior of the resin was characterized by DSC. The test instrument was an American TA Q2000 differential scanning calorimeter. The test was carried out in a nitrogen atmosphere with a gas flow rate of 50 mL / min, a heating rate of 10°C / min, and a temperature range of room temperature to 300°C.

[0046] The thermal stability of the cured product of vinyl ester resin was tested by TGA on a TGA-DSC 1 from Mettler-Toledo with a heating rate of 10°C / min and a nitrogen flow rate of 60 mL / min.

[0047] The glass transition temperature of the modified vinyl ester resin system and the vinyl ester resin cured product of the comparative example was tested by DMA on a DMA-1 of Mettler-Toledo with a frequency of 1 Hz and a heating rate of 5°C / min.

[0048] The impact performance test of the modified vinyl ester resin system and the comparative example of the vinyl ester resin cured product was carried out on a 9050 impact tester of CEAST, Italy, in accordance with the standard ISO 180 "Determination of impact strength of plastics". The impact section was analyzed by SEM using a field emission scanning electron microscope S-3400 of Hitachi, Japan.

[0049] The bending performance test of the modified vinyl ester resin system and the comparative example vinyl ester resin cured product was carried out in accordance with the standard GB / T 2567-2021 "Test method for properties of resin castings" and was tested using Shenzhen Sansi CMT5504 electronic universal testing machine.

[0050] The room temperature and high temperature bending properties and interlaminar shear strength of the modified vinyl ester resin system and the vinyl ester resin cured product of the comparative example were tested with reference to the standards GB / T 1449-2005 "Fiber reinforced plastic bending properties test method" and JC / T773-2010 "Fiber reinforced plastic short beam method for interlaminar shear strength" using the CCSS-44100 electronic universal testing machine of Changchun Institute of Mechanical Science Co., Ltd. The high temperature bending test was carried out after the specimen was kept at 200°C for 10 minutes.

[0051] Example 1

[0052] 80 g of vinyl ester resin and 20 g of BAPPP were added into a 250 mL three-necked flask with a mechanical stirrer and a reflux condenser, and ultrasonically stirred for 15 min at room temperature to form a uniform blended resin BPV-1.

[0053] 1 g of tert-butyl perbenzoate and 0.5 g of cobalt isooctanoate were added to 100 g of BPV-1 blended resin, and the mixture was stirred at room temperature until uniform. The resin was subjected to DSC analysis. The results were as follows: Figure 2 The resin was then poured into a mold coated with a release agent and preheated at 100°C for 10 minutes, and then placed in a high-temperature oven for curing at 60°C / 1h+80°C / 1h+120°C / 1h+200°C / 1h+250°C / 0.5h. After curing, it was naturally cooled to room temperature to obtain a cured product of the blended resin BPV-1, i.e., modified vinyl ester resin system 1.

[0054] The test results of mechanical properties and thermal stability of the modified vinyl ester resin cured product obtained in Example 1 are shown in Table 1.

[0055] Example 2

[0056] 75 g of vinyl ester resin and 25 g of BAPPP were added into a 250 mL three-necked flask with a mechanical stirrer and a reflux condenser, and ultrasonically stirred for 15 min at room temperature to form a uniform blended resin BPV-2.

[0057] 1 g of tert-butyl perbenzoate and 0.5 g of cobalt isooctanoate were added to 100 g of BPV-2 blended resin, and the mixture was stirred at room temperature until uniform. The resin was subjected to DSC analysis. The results were as follows: Figure 2 The resin was then poured into a mold coated with a release agent and preheated at 100°C for 10 minutes, and then placed in a high-temperature oven for curing at 60°C / 1h+80°C / 1h+120°C / 1h+200°C / 1h+250°C / 0.5h. After curing, it was naturally cooled to room temperature to obtain a cured product of the blended resin BPV-2, i.e., modified vinyl ester resin system 2.

[0058] The test results of mechanical properties and thermal stability of the modified vinyl ester resin cured product obtained in Example 2 are shown in Table 1.

[0059] Example 3

[0060] 70 g of vinyl ester resin and 30 g of BAPPP were added into a 250 mL three-necked flask with a mechanical stirrer and a reflux condenser, and ultrasonically stirred for 15 min at room temperature to form a uniform blended resin BPV-3.

[0061] 1 g of tert-butyl perbenzoate and 0.5 g of cobalt isooctanoate were added to 100 g of BPV-3 blended resin, and the mixture was stirred at room temperature until uniform. The resin was subjected to DSC analysis. The results were as follows: Figure 2 The resin was then poured into a mold coated with a release agent and preheated at 100°C for 10 minutes, and then placed in a high-temperature oven for curing at 60°C / 1h+80°C / 1h+120°C / 1h+200°C / 1h+250°C / 0.5h. After curing, it was naturally cooled to room temperature to obtain a cured product of the blended resin BPV-3, i.e., modified vinyl ester resin system 3.

[0062] The test results of mechanical properties and thermal stability of the modified vinyl ester resin cured product obtained in Example 3 are shown in Table 1.

[0063] Example 4

[0064] 75 g of vinyl ester resin and 25 g of BAPPP were added into a 250 mL three-necked flask equipped with a mechanical stirrer and a reflux condenser, and stirred at room temperature for 15 min to form a uniform blended resin BPV-2.

[0065] Add 1.5 g of methyl ethyl ketone peroxide and 0.5 g of cobalt cyclohexane acid to 100 g of BPV-2 blended resin, stir thoroughly at room temperature until uniform, and perform DSC analysis on the resin. The results are as follows: Figure 2 The resin was then poured into a mold coated with a release agent and preheated at 100°C for 10 min, and then placed in a high-temperature oven for curing at 60°C / 1h+80°C / 1h+120°C / 1h+200°C / 1h+250°C / 0.5h. After curing, it was naturally cooled to room temperature to obtain a cured product of the blended resin BPV-4, a modified vinyl ester resin system 4.

[0066] The test results of mechanical properties and thermal stability of the modified vinyl ester resin cured product obtained in Example 4 are shown in Table 1.

[0067] Comparative Example 1

[0068] In order to compare the performance advantages of the modified vinyl ester resins obtained in Examples 1-4 above, a comparative example was designed to be a commercially available vinyl ester resin used for modification without the addition of BPAPP.

[0069] Add 1g of tert-butyl peroxybenzoate and 0.5g of cobalt isooctanoate to 100g of vinyl ester resin, and stir thoroughly at room temperature until uniform. Then pour into a mold coated with a release agent and preheated at 100°C for 20 minutes, let stand at room temperature for 24 hours to pre-cure the resin, and then put it in a high-temperature oven to cure it at 60°C / 1h+80°C / 1h+140°C / 1h. After curing, naturally cool to room temperature to obtain a cured vinyl ester resin.

[0070] The test results of mechanical properties and thermal stability of the vinyl ester resin cured product obtained in Comparative Example 1 are shown in Table 1.

[0071] Table 1 Performance results of the modified vinyl ester resin cured products of Examples 1-4 and the vinyl ester resin cured product of Comparative Example 1.

[0072]

[0073] It can be seen from Table 1 that the modified vinyl ester resins of Examples 1-4 have better bending properties, higher thermal stability and excellent comprehensive performance compared to the vinyl ester resin before modification, especially the impact strength in the examples is higher than that in Comparative Example 1, which shows that BAPPP has the effect of toughening the vinyl ester resin. As shown in Figure 5, the impact section of the vinyl ester resin is a relatively smooth surface, while the impact section of the modified resin is very rough, with complex fracture lines, which is a typical tough fracture surface feature. The above illustrates that the modified vinyl ester resin of the present invention has the advantages of mechanical properties and heat resistance.

[0074] The heat resistance advantage is further demonstrated by preparing T300 carbon fiber composite material with modified resin.

[0075] Example 5

[0076] The T300 carbon fiber composite material was produced using the BPV-3 resin in Example 3 above.

[0077] After adding 1g of tert-butyl peroxybenzoate and 0.5g of cobalt isooctanoate to 100g of BPV-3 resin, the mixture was stirred and ultrasonicated for 15min to form a uniform and transparent glue solution. An appropriate amount of glue solution was taken and evenly applied to each layer of T300 carbon cloth (200mm×150mm) within 30min. 12 layers of carbon cloth were stacked one by one and placed in a metal mold. T300 carbon fiber reinforced modified vinyl ester resin composite material (T300CF / BAPPP / VER) was prepared at 3MPa with a heating program of 60℃ / 1h+80℃ / 1h+120 / 1h+200℃ / 1h+250℃ / 30min. After hot pressing, the composite material plate was cut into the required size for the test according to the standard.

[0078] The mechanical property test results of the T300 carbon fiber reinforced modified vinyl ester resin composite material obtained in Example 5 are shown in Table 2.

[0079] Comparative Example 2

[0080] Design comparison example 2 is a T300 carbon fiber composite material prepared by commercially available vinyl ester resin without adding BAPPP.

[0081] Add 1g of tert-butyl peroxybenzoate and 0.5g of cobalt isooctanoate to 100g of vinyl ester resin, and stir thoroughly at room temperature until uniform. Take an appropriate amount of glue, and evenly apply the glue on each layer of T300 carbon cloth (200mm×150mm) within 30min. Stack 12 layers of carbon cloth one by one and place them in a metal mold. Prepare T300 carbon fiber reinforced vinyl ester resin composite material (T300CF / VER) at 3MPa with a heating program of 60℃ / 1h+80℃ / 1h+120℃ / 1h. After hot pressing, cut the composite board into the required size for testing according to the standard.

[0082] The mechanical property test results of the T300 carbon fiber reinforced vinyl ester resin composite material obtained in Comparative Example 2 are shown in Table 2.

[0083] Table 2 Performance results of the modified vinyl ester resin composite material of Example 5 and the vinyl ester resin composite material of Comparative Example 2.

[0084]

[0085] It can be seen from Table 2 that the modified vinyl ester resin composite material of Example 5 has better mechanical properties than the vinyl ester resin composite material before modification, and has higher mechanical properties at a high temperature of 200° C. This illustrates the superiority of the heat-resistant high-strength and high-toughness vinyl ester resin described herein.

[0086] The above is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any technician familiar with the present invention can make some changes or modify the above technical contents into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of the solution of the present invention.

Claims

1. A method for preparing a heat-resistant high-strength and high-toughness modified vinyl ester resin, characterized in that: The preparation method comprises the following steps: (1) mixing a tetrafunctional compound containing a dipropargyl group and a diallyl group with a vinyl ester resin in a mass ratio of 1:1 to 1:5; (2) simultaneously ultrasonically and mechanically stirring the mixture of step (1) at 25-30° C. to prepare a vinyl ester resin blend; (3) adding 0.1% to 5% of the weight of the resin blend of the curing agent and 0.1% to 1% of the accelerator to the vinyl ester resin blend, stirring until homogeneous, and standing to remove bubbles; (4) pouring the product obtained in step (3) into a mold coated with a release agent, and curing at 60-250° C. to obtain the modified vinyl ester resin system; Wherein: the vinyl ester resin in step (1) is a bisphenol A epoxy vinyl ester resin or a phenolic epoxy vinyl ester resin, and its acid value is lower than 10 mgKOH / g and its room temperature viscosity is lower than 800 mPa s; The tetrafunctional compound containing a dipropargyl group and a diallyl group in step (1) is diallyl bisphenol A dipropargyl ether, and its structural formula is shown in Formula I: Formula I The curing agent used in step (3) is one or a mixture of more than one selected from methyl ethyl ketone peroxide, acetylacetone peroxide, cyclohexanone peroxide, benzoyl peroxide, dilauroyl peroxide, tert-butyl perbenzoate, dibenzoyl peroxide and tert-butyl hydroperoxide; The promoter used in step (3) is one or a mixture of more than one selected from the group consisting of cobalt isooctanoate, cobalt cyclopentadiene cobalt, dicyclopentadiene nickel, nickel acetylacetonate, dimethylaniline and diethylaniline.

2. The method for preparing a modified vinyl ester resin according to claim 1, wherein The vinyl ester resin in step (1) is a phenolic epoxy vinyl ester resin.

3. The method for preparing the modified vinyl ester resin according to claim 1, wherein The ultrasound in step (2) is carried out in an ultrasonic water bath, with a stirring speed of 250 rpm and a stirring time of 10 to 15 minutes.

4. The method for preparing a modified vinyl ester resin according to claim 1, wherein The curing agent in step (3) is methyl ethyl ketone peroxide or tert-butyl perbenzoate, and the amount used is 0.5%-2% of the weight of the vinyl ester resin blend; the accelerator is cobalt isooctanoate or cobalt cyclohexaneate, and the amount used is 0.5% of the weight of the vinyl ester resin blend.

5. The method for preparing the modified vinyl ester resin according to claim 1, characterized in that: Step (3) The temperature of adding the curing agent and the accelerator into the blended resin is 30-50° C., the stirring time is 10-20 min, and the standing time is 10-20 min.

6. The method for preparing the modified vinyl ester resin according to claim 5, characterized in that: The stirring time of step (3) is 10 min and the standing time is 15 min.

7. The method for preparing a modified vinyl ester resin according to claim 1, wherein: The curing method in step (4) is preferably step curing, which is carried out according to the following steps: keeping warm at 60-80°C for 2-4h, keeping warm at 100-200°C for 1-2h, and keeping warm at 200-250°C for 3-5h. After curing, the obtained product is naturally cooled to 25-30°C.

Citation Information

Patent Citations

  • Preparation method of modified vinyl ester resin

    CN117624845A

  • Curable prepreg composition, method for producing the same and method for curing the same

    JP2001294687A

  • Structure of phosphorous-containing functionalized poly(arylene ether) and compositions prepared therefrom

    US20160130406A1

  • Resin composition comprising a specific crosslinking agent

    US20220064342A1

  • Vinyl ester resin composition, composite material containing said composition, and cured product of said composition or composite material

    WO2020066175A1