Method for degrading epoxy anhydride cured product and directly recycling degradation product of epoxy anhydride cured product
By using a catalyst to dissolve the degradation solvent in the epoxy anhydride cured product, it is prepared by regulating the reaction with urea, formaldehyde, furfuryl alcohol, etc., the resulting degradation solution can be directly used for furan resin synthesis, solving the degradation product of epoxy anhydride resin The unused problem has achieved efficient, environmentally friendly and economical degradation and reuse, and improved the tensile strength of the furan resin.
Patent Information
- Application Number
- CN202411129223.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-29
AI Technical Summary
In the prior art, the degradation process of epoxy anhydride resin is complicated and the degradation products are not effectively utilized, which affects the economic and environmental protection of the method.
By soluble catalyst and furfuryl alcohol, degradation solvent is obtained, epoxy anhydride cured substance is added for heating and stirring, and then mixed with urea, formaldehyde and furfuryl alcohol, adjust the pH value and insulating and heating reaction, add silane, and finally obtain a direct use of furan Degradable solution for resin synthesis.
Under mild conditions, the degradation solution contains a large amount of furan ring and hydroxyl bonds, which participate in the curing reaction of furan resin, and improves its tensile strength and quality. The whole process is simple, efficient and pollutant-free. It is produced and has good economicality.
Smart Images

Figure CN119039549A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of solid waste material recovery, and in particular relates to a degradation method of epoxy anhydride solidified material and a direct recovery and utilization method of its degradation products. Background Art
[0002] Epoxy anhydride resin is a material with excellent performance, wide application fields and important value. In the electrical and electronic industry, it is used for insulation packaging of electrical appliances and motors and potting of electronic components, providing guarantee for the safe and stable operation of electronic equipment. In the field of composite materials, the fiberglass and structural composite materials manufactured are key materials in high-tech fields such as aerospace and wind power generation. In the field of coatings and adhesives, its coatings have good corrosion resistance and weather resistance, and its adhesives have excellent bonding properties, meeting the needs of various industries. In civil construction, it is an important material for anti-corrosion, reinforcement and repair.
[0003] However, epoxy anhydride resin is a thermosetting resin, and it is difficult to recycle the material after its service life expires. Currently, it is mainly treated by incineration, landfill, etc., which causes serious environmental pollution and waste of resources. Many works are devoted to solving the recycling and reuse problem of epoxy anhydride resin by chemical degradation. However, some of these methods have complicated degradation processes, some do not provide a method for reusing the degradation products, and some degradation products need to be separated in a complex way before they can be used, which affects the economic efficiency of the method. Therefore, they have not been widely used in actual industry.
[0004] For example, the patent CN111718515A discloses a method for catalyzing the degradation of anhydride-cured epoxy resin, which prepares anhydride-cured epoxy resin, a reaction solvent, and an organic acid catalyst into a degradation system for degradation reaction. After the degradation is completed, hot water is added, fully dissolved and filtered, and the filtrate is evaporated to recover the reaction solvent, curing agent and organic acid catalyst, and the filter cake is the organic phase epoxy resin degradation product. However, the invention patent does not provide a clear use of the filter cake component epoxy resin degradation product on the one hand, and on the other hand, the filtrate still needs to be subjected to a more complicated chemical separation, which affects the economic efficiency of the method.
[0005] Another example is the alcoholysis recovery and re-preparation method of anhydride-cured epoxy resin for electrical equipment disclosed in patent CN116063738A, which places epoxy resin, anhydrous ethanol and alkaline catalyst (such as potassium phosphate solid powder) in a reactor with a polytetrafluoroethylene liner for alcoholysis reaction to obtain degradation products, separates the catalyst by filtering with filter paper, heats and evaporates the ethanol in the solution to obtain degraded epoxy resin, and uses it to replace part of bisphenol A diglycidyl ether to prepare new epoxy resin. The degradation products in this patent also need to go through a complex chemical separation step, which affects the economic efficiency of the method. Summary of the invention
[0006] An object of the present invention is to solve at least the above problems and / or disadvantages and to provide at least the advantages which will be described hereinafter.
[0007] In order to achieve these purposes and other advantages according to the present invention, a method for degrading epoxy anhydride cured material and directly recycling its degradation products is provided, comprising the following steps:
[0008] Step 1, dissolving the catalyst and furfuryl alcohol to obtain a degradation solvent;
[0009] Step 2: adding the epoxy anhydride cured product into a reaction kettle, adding a degradation solvent, heating and stirring to degrade the epoxy anhydride cured product, and obtaining a degradation liquid;
[0010] Step 3: Evenly mix urea, formaldehyde and furfuryl alcohol, then add sodium hydroxide to adjust the pH, keep warm for reaction, cool down, add formic acid to adjust the pH, heat up for reaction, cool down again, add the degradation solution obtained in step 2, then add silane, then adjust the pH with ammonia water, mix and react for a period of time, and then obtain furan resin.
[0011] Preferably, the catalyst is an inorganic base and / or an organic base.
[0012] Preferably, the inorganic base is one or more of sodium hydroxide (NaOH), potassium hydroxide (KOH), barium hydroxide (Ba(OH)2), calcium hydroxide (Ca(OH)2), and ammonia water; the organic base is one or more of 1,5,7-triazabicyclo[4.4.0]dec-5-ene, ethyleneamine, allylamine, DMP-30, and alcoholamine.
[0013] Preferably, in the step 1, the ratio of the catalyst to furfuryl alcohol is 0.2-2 mol:1L, and the concentration of the prepared degradation solvent is 0.2-2M.
[0014] Preferably, in step 2, the epoxy anhydride cured product is an epoxy anhydride cured product of bisphenol A epoxy resin and methyltetrahydrophthalic anhydride or methylhexahydrophthalic anhydride, and the mass ratio of the epoxy anhydride cured product to the degradation solvent is 1:1 to 1:10.
[0015] Preferably, in step 2, the heating and stirring degradation temperature is 50° C. to 170° C., and the degradation time is 0.5 to 6 hours.
[0016] Preferably, in the step three, the mass ratio of urea, formaldehyde, furfuryl alcohol and degradation liquid is 35:30-200:50-200:10-1000, and the formaldehyde is solid formaldehyde or formaldehyde solution. When formaldehyde solution is used, it needs to be converted according to concentration.
[0017] Preferably, in step three, sodium hydroxide is used to adjust the pH to 9.0-9.2, the reaction is carried out at 88-90° C. for 60 min, and then the temperature is lowered to below 60° C.
[0018] Preferably, in step three, after cooling, formic acid is used to adjust the pH to 4.0-4.2, the temperature is raised to 98-100° C. for reaction for 60 min, and then the temperature is lowered to below 50° C. for a second time.
[0019] Preferably, in step three, the silane is one or more of N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane (KH602), γ-aminopropyltriethoxysilane (KH550), and N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane (KH-792), and the amount of silane is 0.2% to 0.6% of the total amount of urea, formaldehyde, furfuryl alcohol and degradation liquid. The pH is adjusted to 8.5 to 9.0 with ammonia water, and the mixing reaction is carried out for 10 minutes.
[0020] The present invention at least includes the following beneficial effects: the present invention realizes efficient degradation of epoxy anhydride cured products under mild conditions; the degradation liquid does not need to be separated and can be directly used for furan resin synthesis, and the molecules of the degradation liquid contain a large number of furan rings and a large number of hydroxyl bonds. Both chemical bonds can participate in the curing reaction of the furan resin, and the introduction of macromolecules in the degradation liquid improves the toughness of the furan resin, so the furan resin prepared by the degradation liquid has better tensile strength, improves the quality of the furan resin, and has improved tensile strength compared with the original furan resin; the entire degradation and recycling process is simple and efficient, no pollutants are generated, and it is environmentally friendly and economical.
[0021] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 is the synthesis formula of epoxy anhydride curing material;
[0023] Figure 2 The decomposition equation of the epoxy anhydride cured product is shown in FIG. DETAILED DESCRIPTION
[0024] The present invention is further described in detail below in conjunction with the accompanying drawings so that those skilled in the art can implement the invention with reference to the description.
[0025] Example 1
[0026] A method for degrading epoxy anhydride cured product and directly recycling its degradation products comprises the following steps:
[0027] Step 1: Prepare a degradation solvent with a concentration of 1 M NaOH by dissolving 40 g NaOH in 1 L furfuryl alcohol;
[0028] Step 2: Add 3 kg of bisphenol A epoxy resin and epoxy anhydride cured by methyltetrahydrophthalic anhydride into a reaction kettle, add 20 kg of degradation solvent, heat to 100 ° C and stir for 4 hours to degrade the epoxy anhydride cured product, and the obtained degradation liquid is directly used for the synthesis of furan resin;
[0029] Step 3: Use the degradation liquid to partially synthesize the furan resin, the method is as follows: 35g urea, 100g formaldehyde, and 100g furfuryl alcohol are mixed evenly, the pH is adjusted to 9.0 with sodium hydroxide, and the mixture is kept at 90°C for 60min; after the reaction is completed, the temperature is lowered to below 60°C, the pH is adjusted to 4.0 with formic acid, the temperature is raised to 100°C, and the reaction is carried out for 60min; the temperature is lowered to below 50°C for a second time, 480g degradation liquid is added, 3.5g KH602 is added, the pH is adjusted to 9.0 with aqueous ammonia, and the mixture is mixed for 10 minutes to obtain a furan resin with a nitrogen content of 1%.
[0030] Example 2
[0031] A method for degrading epoxy anhydride cured product and directly recycling its degradation products comprises the following steps:
[0032] Step 1: Prepare a degradation solvent with a concentration of 0.5 M KOH by dissolving 28 g KOH in 1 L furfuryl alcohol;
[0033] Step 2: Add 2 kg of bisphenol A epoxy resin and epoxy anhydride cured by methyltetrahydrophthalic anhydride into a reaction kettle, add 20 kg of degradation solvent, heat to 80° C. and stir for 5 h to degrade the epoxy anhydride cured product, and the obtained degradation liquid is directly used for the synthesis of furan resin;
[0034] Step 3: partially synthesizing furan resin using the degradation liquid, the method is consistent with Example 1.
[0035] Example 3
[0036] A method for degrading epoxy anhydride cured product and directly recycling its degradation products comprises the following steps:
[0037] Step 1: Prepare a degradation solvent with a concentration of 0.5 M NaOH by dissolving 20 g NaOH in 1 L furfuryl alcohol;
[0038] Step 2: Add 2 kg of bisphenol A epoxy resin and epoxy anhydride cured by methyl hexahydrophthalic anhydride into a reaction kettle, add 20 kg of degradation solvent, heat to 160° C. and stir for 1.5 h to degrade the epoxy anhydride cured product, and the obtained degradation liquid is directly used for the synthesis of furan resin;
[0039] Step 3: partially synthesizing furan resin using the degradation liquid, the method is consistent with Example 1.
[0040] Example 4
[0041] A method for degrading epoxy anhydride cured product and directly recycling its degradation products comprises the following steps:
[0042] Step 1: Prepare a degradation solvent with a concentration of 2M NaOH by dissolving 80g NaOH in 1L furfuryl alcohol;
[0043] Step 2: Add 10 kg of bisphenol A epoxy resin and epoxy anhydride cured by methyltetrahydrophthalic anhydride into a reaction kettle, add 20 kg of degradation solvent, heat to 80°C and stir for 8 hours to degrade the epoxy anhydride cured product, and the obtained degradation liquid can be directly used for the synthesis of furan resin.
[0044] Step 3: partially synthesizing furan resin using the degradation liquid, the method is consistent with Example 1.
[0045] Example 5
[0046] A method for degrading epoxy anhydride cured product and directly recycling its degradation products comprises the following steps:
[0047] Step 1: Prepare a degradation solvent with a concentration of 1.5 M KOH by dissolving 84 g KOH in 1 L furfuryl alcohol;
[0048] Step 2: Add 1 kg of bisphenol A epoxy resin and epoxy anhydride cured by methyltetrahydrophthalic anhydride into a reaction kettle, add 20 kg of degradation solvent, heat to 160° C. and stir for 0.5 h to degrade the epoxy anhydride cured product, and the obtained degradation liquid is directly used for the synthesis of furan resin;
[0049] Step 3: partially synthesizing furan resin using the degradation liquid, the method is consistent with Example 1.
[0050] Example 6
[0051] A method for degrading epoxy anhydride cured product and directly recycling its degradation products comprises the following steps:
[0052] Step 1: 35 g of 1,5,7-triazabicyclo[4.4.0]dec-5-ene (TBD) and 1 L of furfuryl alcohol are dissolved in each other to prepare a degradation solvent with a concentration of 0.25 M TBD;
[0053] Step 2: Add 4 kg of bisphenol A epoxy resin and epoxy anhydride cured by methyltetrahydrophthalic anhydride into a reaction kettle, add 20 kg of degradation solvent, heat to 160° C. and stir for 0.5 h to degrade the epoxy anhydride cured product. The degradation liquid can also be directly used for the synthesis of furan resin without separation steps;
[0054] Step 3: partially synthesizing furan resin using the degradation liquid, the method is consistent with Example 1.
[0055] Comparative Example 1
[0056] The furan resin is prepared by a conventional method without using a degradation solution. The specific method is as follows:
[0057] Mix 35g urea, 100g formaldehyde and 100g furfuryl alcohol evenly, adjust the pH to 9.0 with sodium hydroxide, and react at 90°C for 60min; after the reaction is completed, cool to below 60°C, adjust the pH to 4.0 with formic acid, heat to 100°C, and react for 60min; cool to below 50°C for a second time, add 540g furfuryl alcohol, add 3.5g KH602, adjust the pH to 9.0 with ammonia water, mix and react for 10 minutes, and you can get a furan resin with a nitrogen content of 1%.
[0058] The furan resin prepared in Examples 1 to 6 and Comparative Example 1 was used to bond the foundry sand, and the tensile strength of the furan resin was tested using the method of GB / T2684. The results are shown in Table 1:
[0059] Table 1 Example and Comparative Example Furan resin tensile strength
[0060] Tensile strength / MPa Example 1 2.04 Example 2 2.13 Example 3 1.89 Example 4 2.10 Example 5 1.78 Example 6 1.86 Comparative Example 1 1.68
[0061] It can be seen from Table 1 that under comparable conditions, the tensile strength of the furan resin containing the degradation liquid prepared by the present invention is higher than that of the conventional furan resin. Figure 1 is the synthesis formula of epoxy anhydride curing material, Figure 2 The equation for the degradation of epoxy anhydride solidified material by furfuryl alcohol shows that the degradation product is composed of two parts (a) and (b), wherein the (a) molecule contains a large number of furan rings, and the (b) molecule contains a large number of hydroxyl bonds. Both chemical bonds can participate in the curing reaction of the furan resin, and the introduction of macromolecules in the degradation liquid improves the toughness of the furan resin, so the furan resin prepared by the degradation liquid has better tensile strength and improves the quality of the furan resin. It can be seen that the degradation liquid participates in the curing reaction of the furan resin, and the furan resin modified by the macromolecules in the degradation liquid has better tensile strength. The present invention realizes the degradation of epoxy anhydride solidified material by a simple and efficient method, and the degradation product can be directly utilized without complicated separation steps, and no three wastes are generated, which is environmentally friendly, efficient, and has good economy.
[0062] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and implementation modes. They can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and the illustrations shown and described herein.
Claims
1. A method for degrading epoxy anhydride cured products and directly recycling their degradation products, characterized in that: The following steps are involved: Step 1, dissolving the catalyst and furfuryl alcohol to obtain a degradation solvent; Step 2: adding the epoxy anhydride cured product into a reaction kettle, adding a degradation solvent, heating and stirring to degrade the epoxy anhydride cured product to obtain a degradation liquid; Step 3: Evenly mix urea, formaldehyde and furfuryl alcohol, then add sodium hydroxide to adjust the pH, keep warm for reaction, cool down, add formic acid to adjust the pH, heat up for reaction, cool down again, add the degradation solution obtained in step 2, then add silane, then adjust the pH with ammonia water, mix and react for a period of time, and then obtain furan resin.
2. The method for degrading epoxy anhydride cured product and directly recycling its degradation products according to claim 1, characterized in that: In the step 1, the catalyst is an inorganic base and / or an organic base.
3. The method for degrading epoxy anhydride cured product and directly recycling its degradation products according to claim 2, characterized in that: The inorganic base is one or more of sodium hydroxide, potassium hydroxide, barium hydroxide, calcium hydroxide and ammonia water; the organic base is one or more of 1,5,7-triazabicyclo[4.4.0]dec-5-ene, ethyleneamine, allylamine, DMP-30 and alcoholamine.
4. The method for degrading epoxy anhydride cured product and directly recycling its degradation product according to claim 1, characterized in that: In the step 1, the usage ratio of the catalyst to furfuryl alcohol is 0.2-2 mol:1L, and the concentration of the prepared degradation solvent is 0.2-2M.
5. The method for degrading epoxy anhydride cured product and directly recycling its degradation product according to claim 1, characterized in that: In the step 2, the epoxy anhydride cured product is an epoxy anhydride cured product of bisphenol A epoxy resin and methyltetrahydrophthalic anhydride or methylhexahydrophthalic anhydride, and the mass ratio of the epoxy anhydride cured product to the degradation solvent is 1:1 to 1:
10.
6. The method for degrading epoxy anhydride cured product and directly recycling its degradation products according to claim 1, characterized in that: In the step 2, the heating and stirring degradation temperature is 50° C. to 170° C., and the degradation time is 0.5 to 6 hours.
7. The method for degrading epoxy anhydride cured product and directly recycling its degradation product according to claim 1, characterized in that: In the step 3, the mass ratio of urea, formaldehyde, furfuryl alcohol and degradation liquid is 35:30-200:50-200:10-1000, and the formaldehyde is solid formaldehyde or formaldehyde solution.
8. The method for degrading epoxy anhydride cured product and directly recycling its degradation product according to claim 1, characterized in that: In the step 3, the pH is adjusted to 9.0-9.2 with sodium hydroxide, the reaction is carried out at 88-90° C. for 60 minutes, and then the temperature is lowered to below 60° C.
9. The method for degrading epoxy anhydride cured product and directly recycling its degradation product according to claim 1, characterized in that: In the step 3, after cooling, formic acid is used to adjust the pH to 4.0-4.2, the temperature is raised to 98-100° C. for reaction for 60 min, and then the temperature is lowered to below 50° C. for a second time.
10. The method for degrading epoxy anhydride cured product and directly recycling its degradation product according to claim 1, characterized in that: In the step three, the silane is one or more of N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane, γ-aminopropyltriethoxysilane, and N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane. The amount of silane used is 0.2% to 0.6% of the total amount of urea, formaldehyde, furfuryl alcohol and degradation liquid. The pH is adjusted to 8.5 to 9.0 with ammonia water, and the mixing reaction is carried out for 10 minutes.
Citation Information
Cited By
Degradation reagent of anhydride cured epoxy resin composite material, degradation method and application of degradation product
CN120535829A