Preparation method of modified epoxy light-cured resin
By reacting polyetheramine with acryloyl chloride to form an amine-modified prepolymer and extending chain with a polymer inhibitor, the existing modified epoxy acrylate has solved the problem of high viscosity and poor toughness, and low viscosity and high toughness are prepared. The modified epoxy photocuring resin maintains hardness and heat resistance, while improving the flexibility and gloss of the cured film.
Patent Information
- Application Number
- CN202411105201.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-29
AI Technical Summary
The existing modified epoxy acrylates have shortcomings in improving the toughness and yellowing resistance of the cured film, resulting in high viscosity and poor toughness of the cured film.
Polyetheramine and acryloyl chloride react under the action of acid binding agent to form polyetheracrylamide, and then ring-opening reaction with epoxy resin to form an amine-modified prepolymer, and chain-extending reaction with polymer inhibitor to prepare Modified epoxy photocuring resin.
The modified epoxy photocuring resin with low viscosity and good toughness is achieved, and the hardness and heat resistance of the bisphenol A epoxy resin are maintained, while improving the flexibility and gloss of the cured film.
Smart Images

Figure BDA0004990550060000031 
Figure BDA0004990550060000041
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of photocurable resins, and in particular relates to a method for preparing a modified epoxy photocurable resin. Background Art
[0002] Ultraviolet (UV) curing technology is a new technology with the advantages of high production efficiency, low VOC emissions, low energy consumption, and good performance of cured films. It is widely used in the fields of coatings, inks, adhesives, etc. Photocurable resins (also called oligomers) are a type of photosensitive resin with relatively low molecular weight. They have a photocurable reaction group and are the main body in the formulation of photocurable materials. Their performance basically determines the main properties of the cured film.
[0003] Epoxy acrylate is the most widely used and largest amount of photocurable oligomer. According to different structural types, it can be divided into bisphenol A epoxy acrylate, novolac epoxy acrylate, etc. Bisphenol A epoxy acrylate molecules contain benzene rings, and the resin as a whole has good heat resistance, strength and hardness. At the same time, the hydroxyl group of the side chain is conducive to improving adhesion. In addition, the raw materials of bisphenol A epoxy resin are widely available and cheap, so it is widely used in UV wood paint, paper varnish, plastics and other fields. However, bisphenol A epoxy acrylate also has some defects: the cured film has poor flexibility, high brittleness, poor yellowing resistance, etc. In order to improve these defects, many scientific researchers have modified its structure to obtain modified epoxy acrylate.
[0004] Chinese patent application No. 201210219448.3 discloses a modified epoxy acrylate and a preparation method thereof, which uses a mixture of acrylic acid or hydroxy acrylate and dibasic acid anhydride, epoxy resin, catalyst, and inhibitor for "one-pot cooking". The resulting product is light green. This method has the advantage of short reaction time, but the product is darker in color and cannot be water-white and transparent. In addition, due to the continuous chain extension reaction of acid anhydride and epoxy group during the reaction, the molecular weight increases, the viscosity is high, and the toughness of the cured film is poor.
[0005] Chinese patent application No. 202110585162.6 discloses a method for preparing modified epoxy acrylate, which first reacts hydroxy acrylate with anhydride, then reacts with epoxy resin for ring-opening reaction, and finally reacts with halogenated phosphite under the action of an acid binding agent to obtain the final product. The modified epoxy acrylate prepared by this method has improved yellowing resistance, but the rigidity of the molecular structure is still strong, resulting in high viscosity and relatively poor toughness of the cured film. Summary of the invention
[0006] Purpose of the invention: The purpose of the present invention is to overcome the deficiencies in the prior art and provide a novel preparation method for preparing a modified epoxy photocurable resin with low viscosity and good toughness.
[0007] Technical solution: In order to achieve the above invention objectives, the technical solution adopted by the present invention is:
[0008] A method for preparing a modified epoxy photocurable resin comprises the following steps:
[0009] (1) using polyetheramine and acryloyl chloride to react under the action of an acid binding agent to obtain polyether acrylamide;
[0010] (2) using epoxy resin to first undergo a ring-opening reaction with an excess of primary amine to obtain an amine-modified prepolymer;
[0011] (3) The polyether acrylamide and the amine-modified prepolymer undergo a chain extension reaction, and a certain amount of polymerization inhibitor is added to obtain a modified epoxy photocurable resin.
[0012] As a preferred embodiment, in the method for preparing the modified epoxy photocurable resin described above, the polyetheramine in step (1) is selected from one or more of Huntsman's polyetheramines JEFFAMINE D-230, D-400, ED-600, and ED-900; and the acid binding agent is selected from one or more of triethylamine, tri-n-butylamine, 4-dimethylaminopyridine, and pyridine.
[0013] As a preferred embodiment, the preparation method of the modified epoxy light-curing resin described above, the synthesis method of the polyether acrylamide described in step (1) is: polyether amine, acid binding agent and toluene are mixed in a certain proportion, placed in an ice water bath, acryloyl chloride is slowly added dropwise, after 1 to 2 hours of dripping, the temperature is slowly raised to room temperature and the reaction is continued for 12 hours, saturated salt water is added for washing three times, and toluene is removed under vacuum conditions to obtain the desired product. The molar ratio of polyether amine to acryloyl chloride is controlled to be 0.5:1.03 to 0.5:1.08, the molar ratio of acryloyl chloride to acid binding agent is 1:1, toluene accounts for 20 to 50% of the total mass of the material, and the salt water used for each washing accounts for 20 to 40% of the total mass of the material.
[0014] As a preferred embodiment, in the method for preparing a modified epoxy photocurable resin described above, the epoxy resin in step (2) is selected from one or more of SM828, Nan Ya 128, and Dow DER331 of Jiangsu Sanmu Chemical Co., Ltd.; and the primary amine is selected from one or more of 1-propylamine, 1-butylamine, and 1-hexylamine.
[0015] As a preferred embodiment, in the above-mentioned method for preparing a modified epoxy photocurable resin, the synthesis method of the amine-modified prepolymer in step (2) is as follows: a certain mass of primary amine is placed in a reaction flask, and epoxy resin is slowly added dropwise for about 1 hour, and the reaction temperature is controlled not to exceed 60°C using a water bath, and then the reaction is continued at 50-60°C for 6-8 hours. The molar ratio of the amino group of the primary amine to the epoxy group of the epoxy resin is controlled to be 1:1 to 1.05:1.
[0016] As a preferred embodiment, in the above-mentioned method for preparing a modified epoxy photocurable resin, the polymerization inhibitor in step (3) is selected from one or more of p-hydroxyanisole, hydroquinone, and 3,5-di-tert-butyl-4-hydroxytoluene.
[0017] As a preferred embodiment, in the preparation method of the modified epoxy photocurable resin described above, the synthesis method of the modified epoxy photocurable resin described in step (3) is: adding polyether acrylamide and amine-modified prepolymer into a reaction bottle in a certain proportion, adding an inhibitor, slowly heating to 60-65° C. and reacting for 10 hours, controlling the molar ratio of polyether acrylamide to amine-modified prepolymer to be 3.0:1-1.5:1, and the inhibitor accounts for 0.05-0.2% of the total mass of the material.
[0018] The beneficial effects of the present invention are:
[0019] Bisphenol A epoxy acrylate is a photocurable resin with the largest usage. Although it has the advantages of high hardness, fast curing, good heat resistance, etc., it also has the defects of poor toughness and high viscosity. In order to retain its advantages to the greatest extent and improve the defects, the present invention proposes a preparation method of a modified epoxy photocurable resin. The modified epoxy photocurable resin prepared by the method has the advantages of low viscosity and good toughness. DETAILED DESCRIPTION
[0020] Example 1
[0021] A modified epoxy light-curing resin, the preparation method comprising the following steps:
[0022] (1) 115 g of Huntsman's polyetheramine JEFFAMINE D-230, 211 g of toluene and 106.3 g of triethylamine were placed in a reaction flask, cooled using an ice-water bath, 95 g of acryloyl chloride was slowly added dropwise over 2 hours, the temperature was slowly raised to room temperature, the reaction was continued for 12 hours, 264 g of saturated brine was added for washing, the process was repeated three times, and toluene was removed under reduced pressure to obtain polyether acrylamide 1;
[0023] (2) 149.1 g of 1-butylamine was placed in a reaction flask, and 372 g of epoxy resin SM828 produced by Jiangsu Sanmu Chemical Co., Ltd. was slowly added over 1 hour. A water bath was used to cool the reaction temperature to a maximum of 60° C., and the temperature was slowly raised to 55° C. and the reaction was continued for 8 hours to obtain an amine-modified prepolymer 1;
[0024] (3) 676 g of polyether acrylamide 1, 518.2 g of amine-modified prepolymer 1 and 1.8 g of p-hydroxyanisole were placed in a reaction flask, slowly heated to 60° C. and reacted for 10 hours to obtain a modified epoxy photocurable resin 1.
[0025] Example 2
[0026] A modified epoxy light-curing resin comprises the following steps:
[0027] (1) 200 g of Huntsman polyetheramine JEFFAMINE D-400, 330 g of toluene and 198.3 g of tri-n-butylamine were placed in a reaction flask, cooled using an ice-water bath, 96.8 g of acryloyl chloride was slowly added dropwise, and the mixture was completely added within 1.5 hours. The mixture was slowly warmed to room temperature, and the reaction was continued for 12 hours. 413 g of saturated brine was added for washing, and the reaction was repeated three times. Toluene was removed under reduced pressure to obtain polyether acrylamide 2;
[0028] (2) 121.7 g of 1-propylamine was placed in a reaction flask, and 372 g of epoxy resin Nan Ya 128 produced by Jiangsu Sanmu Chemical Co., Ltd. was slowly added over 1 hour, and the temperature was cooled in a water bath to control the reaction temperature to be no higher than 60° C., and then the temperature was slowly raised to 55° C. and the reaction was continued for 8 hours to obtain amine-modified prepolymer 2;
[0029] (3) 1117.6 g of polyether acrylamide 2, 490.2 g of amine-modified prepolymer 2 and 1.6 g of hydroquinone were placed in a reaction flask, slowly heated to 60° C. and reacted for 10 hours to obtain a modified epoxy photocurable resin 2.
[0030] Example 3
[0031] A modified epoxy light-curing resin comprises the following steps:
[0032] (1) 300 g of Huntsman's polyetheramine JEFFAMINE ED-600, 319 g of toluene and 83.1 g of pyridine were placed in a reaction flask, cooled using an ice-water bath, 95 g of acryloyl chloride was slowly added dropwise over 2 hours, the temperature was slowly raised to room temperature, the reaction was continued for 12 hours, 398 g of saturated brine was added for washing, the process was repeated three times, and toluene was removed under reduced pressure to obtain polyether acrylamide 3;
[0033] (2) 206.4 g of 1-hexylamine was placed in a reaction flask, and 372 g of Dow DER331 epoxy resin produced by Jiangsu Sanmu Chemical Co., Ltd. was slowly added over 1 hour. A water bath was used to cool the reaction temperature to a maximum of 60° C., and the temperature was slowly raised to 55° C. to continue the reaction for 8 hours to obtain an amine-modified prepolymer 3.
[0034] (3) 1486.8 g of polyether acrylamide 3, 574.4 g of amine-modified prepolymer 3 and 4.1 g of 3,5-di-tert-butyl-4-hydroxytoluene were placed in a reaction flask, slowly heated to 60° C. and reacted for 10 hours to obtain a modified epoxy photocurable resin 3.
[0035] Example 4 Performance Test Example
[0036] The modified epoxy photocurable resin prepared in the above Examples 1 to 3, modified epoxy acrylate SM6100D (produced by Jiangsu Sanmu Chemical Co., Ltd.), and photoinitiator 1173 (produced by Jiangsu Sanmu Chemical Co., Ltd.) were prepared according to the formula in Table 1 to obtain a photocurable varnish.
[0037] Table 1 Light-curing varnish formulation
[0038]
[0039]
[0040] Take the varnish sample prepared in Table 1, and use a wire rod to coat it on a glass plate to obtain a coating with a thickness of about 25 microns. Then irradiate it with a mercury lamp light source to measure the viscosity of the varnish, the number of machine passes to achieve surface dryness, the flexibility and gloss of the cured film, etc. The results are shown in Table 2.
[0041] Table 2 Comparison of properties of light-cured varnish films
[0042] 1# 2# 3# 4# Viscosity (cps / 25℃) 35000 26000 28000 82000 Number of times to reach surface dryness 3 3 3 3 Flexibility 1 1 1 3 Gloss (60°) 96 95 93 94
[0043] The flexibility is tested according to the method described in the national standard GB / T 1731-1993 "Determination of paint film flexibility".
[0044] The gloss is tested according to the method described in the national standard GB / T 9754-2007 "Paints and varnishes, determination of 20°, 60° and 85° specular gloss of paint films without metallic pigments".
[0045] The above experimental results show that compared with conventional modified epoxy acrylate, the modified epoxy photocurable resin prepared by the method of the present invention has lower viscosity and better flexibility. At the same time, the number of machine passes and glossiness of the two to achieve surface dryness are basically the same.
Claims
1. A method for preparing a modified epoxy photocurable resin, characterized in that: The following steps are involved: (1) using polyetheramine and acryloyl chloride to react under the action of an acid binding agent to obtain polyether acrylamide; (2) using epoxy resin to first react with excess primary amine to obtain an amine-modified prepolymer; (3) The polyether acrylamide and the amine-modified prepolymer undergo a chain extension reaction, and a certain amount of polymerization inhibitor is added to obtain a modified epoxy photocurable resin.
2. The method for preparing a modified epoxy photocurable resin according to claim 1, characterized in that: In step (1), the polyetheramine is selected from one or more of Huntsman's polyetheramines JEFFAMINE D-230, D-400, ED-600, and ED-900; and the acid binding agent is selected from one or more of triethylamine, tri-n-butylamine, 4-dimethylaminopyridine, and pyridine.
3. The method for preparing a modified epoxy photocurable resin according to claim 1, characterized in that: The synthesis method of the polyether acrylamide in step (1) is as follows: polyetheramine, acid binding agent and toluene are mixed in a certain proportion, placed in an ice water bath, acryloyl chloride is slowly added dropwise, and after the addition is completed in 1 to 2 hours, the mixture is slowly heated to room temperature and reacted for 12 hours, saturated salt water is added for washing three times, and toluene is removed under vacuum conditions to obtain the desired product. The molar ratio of polyetheramine to acryloyl chloride is controlled to be 0.5:1.03 to 0.5:1.08, the molar ratio of acryloyl chloride to the acid binding agent is 1:1, toluene accounts for 20 to 50% of the total mass of the material, and the salt water used for each washing accounts for 20 to 40% of the total mass of the material.
4. The method for preparing a modified epoxy photocurable resin according to claim 1, characterized in that: In step (2), the primary amine is selected from one or more of 1-propylamine, 1-butylamine and 1-hexylamine.
5. The method for preparing a modified epoxy photocurable resin according to claim 1, characterized in that: The synthesis method of the amine-modified prepolymer in step (2) is as follows: a certain mass of primary amine is placed in a reaction flask, epoxy resin is slowly added dropwise, the addition is completed within 1 hour, the reaction temperature is controlled not to exceed 60° C. using a water bath, and then the reaction is continued at 50-60° C. for 6-8 hours.
6. The method for preparing a modified epoxy photocurable resin according to claim 5, characterized in that: Step (2) controls the molar ratio of the amino group of the primary amine to the epoxy group of the epoxy resin to be 1:1 to 1.05:
1.
7. The method for preparing a modified epoxy photocurable resin according to claim 1, characterized in that: The inhibitor in step (3) is selected from one or more of p-hydroxyanisole, hydroquinone, and 3,5-di-tert-butyl-4-hydroxytoluene.
8. The method for preparing a modified epoxy photocurable resin according to claim 1, characterized in that: The synthesis method of the modified epoxy light-curing resin in step (3) is as follows: polyether acrylamide and amine-modified prepolymer are added into a reaction bottle in a certain proportion, an inhibitor is added, and the temperature is slowly raised to 60-65° C. to react for 10 hours.
9. The method for preparing a modified epoxy photocurable resin according to claim 8, characterized in that: In step (3), the molar ratio of polyether acrylamide to amine-modified prepolymer is controlled to be 3.0:1 to 1.5:1, and the inhibitor accounts for 0.05 to 0.2% of the total mass of the materials.
Citation Information
Cited By
Anti-corrosion coating for submarine conveying pipeline and preparation process of anti-corrosion coating
CN120648329A
Film-forming resin and preparation method thereof, resin composition and solder resist dry film
CN121554634A