Indole-2, 3-dione-based intrinsic microporous polymer and application thereof in preparation of ion solvated membrane and hydrogen production of alkaline water electrolyzer
By introducing indole-2,3-dione self-porous polymer and pore filling technology into ionic solvated films, the problems of insufficient chemical stability and mechanical strength of the existing films are solved, and higher electrolysis is achieved Performance and service life have promoted the development of alkaline water electrolytic cells.
Patent Information
- Application Number
- CN202411267372.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-11-29
AI Technical Summary
The existing ion solvated films have problems such as insufficient chemical stability and poor ion transport capability in alkaline water electrolytic cells, which affect the electrolytic performance.
Indole-2,3-dione is used as the backbone of self-porous polymers, and synthesized by superacid catalytic polymerization method, rigid microporous units are introduced to improve the chemical stability and mechanical properties of the polymer, and porous through PE The separator serves as a substrate and a support layer to prepare a pore-filled ion solvated film.
It significantly improves the chemical stability and mechanical stability of the membrane, enhances the ion transport capability, improves the electrolytic performance and service life, and promotes the development of alkaline water electrolytic cells.
Smart Images

Figure CN119039574A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of alkaline water electrolyzers and ion solvation membranes, and specifically relates to a self-microporous polymer based on indole-2,3-dione and its application in the preparation of ion solvation membranes and hydrogen production in alkaline water electrolyzers. Background Art
[0002] Hydrogen is one of the ideal energy sources in the 21st century. As a renewable secondary energy source, it has the advantages of abundant resources, high calorific value and environmental friendliness. Hydrogen production by water electrolysis is a zero-emission and reliable industrial application technology. Water electrolysis mainly includes alkaline water electrolysis (AWE), proton exchange membrane water electrolysis (PEMWE) and water electrolysis based on solid oxide electrolyzers. Among them, AWE is the most mature and lowest-cost method.
[0003] Alkaline water electrolysis refers to the process of producing hydrogen by electrolysis of water in an alkaline electrolyte environment. The electrolyte is generally a 30% mass concentration KOH solution or a 26% mass concentration NaOH solution. Alkaline electrolyzers are mainly composed of electrodes, catalysts and membranes. There are many ways to reduce the cost of hydrogen production by AWE, such as reducing material costs, increasing operating pressure and temperature, developing efficient catalysts, designing zero-gap membrane electrodes, and exploring high-performance membranes. Among these methods, developing high-performance, low-cost membranes is considered to be one of the most effective strategies. In recent years, the goals for AWE membranes are low area resistance, excellent hydrophilicity, high bubble point pressure, excellent stability in 30wt% KOH solution at 80°C, simple preparation, good mechanical properties and most importantly, high electrolytic performance. Representative membranes such as polyphenylene sulfide (PPS) have been used on a large scale in alkaline electrolyzers, but due to high area resistance, the electrolytic performance is still low.
[0004] Ionic solvation membranes (ISMs) have polar or ionizable groups on the polymer main chain or side chain, such as imidazole and benzimidazole. ISMs absorb electrolytes through these groups, forming a uniform morphology without obvious phase separation structure. Ion transfer is achieved by the absorption and presence of electrolytes. As a new type of diaphragm for alkaline water electrolyzers, ISMs currently have problems such as insufficient chemical stability and poor ion transfer capacity. Summary of the invention
[0005] In view of the problems existing in the above-mentioned prior art, the present invention provides a self-microporous polymer based on indole-2,3-dione and its application in the preparation of ion solvation membrane and hydrogen production in alkaline water electrolyzer.
[0006] The present invention synthesizes a self-microporous polymer main chain containing an indole ketone structure by a superacid catalytic polymerization method, improves the chemical stability of the polymer, solves the problem of poor chemical stability of the ion solvation membrane, and introduces a rigid microporous unit, so that the resulting polymer has a larger free volume while having excellent film-forming properties, which can improve the ion transmission capacity. In addition, the pore-filled ion solvation membrane uses a PE porous diaphragm as a substrate and a supporting layer, which enhances the mechanical properties of the diaphragm. Therefore, the self-microporous polymer based on indole-2,3-dione and its ion solvation membrane, and the pore-filled ion solvation membrane are used as the diaphragm of AWE, which can improve the chemical stability and mechanical stability of the membrane and improve the ion transmission capacity. This research has not been reported in the literature.
[0007] The present invention is based on a self-microporous polymer of indole-2,3-dione, and its general structure is shown in the following formula I:
[0008] A is selected from the following groups:
[0009] *Indicates the connection location.
[0010] n represents the number of repeating units, i.e., the degree of polymerization, 100≤n≤1000.
[0011] The method for preparing a self-microporous polymer based on indole-2,3-dione of the present invention comprises the following steps: Dissolve the twisted rigid monomer and indole-2,3-dione in dichloromethane and trifluoroacetic acid (the volume of trifluoroacetic acid is 0.5 to 1 times the volume of dichloromethane), add trifluoromethanesulfonic acid, and react at room temperature for 0.5 to 24 hours until the viscosity of the polymerization reaction system is relatively high (the viscosity is evaluated by the rotation speed. The lowest viscosity requires a rotation speed of >1000rpm, and the liquid in the system will not splash), slowly pour the reaction solution into water to precipitate the polymer, then wash and dry it several times to obtain a self-microporous polymer based on indole-2,3-dione.
[0012] The torsionally rigid monomer is selected from the compounds of the following structures: .
[0013] The molar ratio of the twisted rigid monomer to indole-2,3-dione is 1:1; the total mass volume concentration of the twisted rigid monomer and indole-2,3-dione in the solvent dichloromethane and trifluoroacetic acid is 10-25g / 100mL; the ratio of the total molar amount of the twisted rigid monomer and indole-2,3-dione to the molar amount of trifluoromethanesulfonic acid is 1:(1-10).
[0014] The method for preparing a self-microporous ion solvation membrane using the self-microporous polymer based on indole-2,3-dione comprises the following steps: The indole-2,3-dione-based self-microporous polymer is dissolved in an organic solvent to obtain a casting solution; the casting solution is used to cast a film and dry it, the film is peeled off, and immersed in a 15-40wt% KOH solution at 80°C for more than three days for sufficient ion exchange, and then the film is taken out and the excess solution on the surface is wiped off, so as to obtain a self-microporous ion solvated membrane.
[0015] The organic solvent is selected from dimethyl sulfoxide and N-methylpyrrolidone, and the mass concentration of the casting solution is controlled at 5-10 wt%.
[0016] The self-microporous ion solvation membrane of the present invention is used as a membrane electrode diaphragm material in hydrogen production in an alkaline water electrolyzer.
[0017] The method of using the self-microporous polymer pores based on indole-2,3-dione to fill the ion solvation membrane comprises the following steps: The indole-2,3-dione-based self-microporous polymer is dissolved in an organic solvent to obtain a casting solution; the casting solution is cast on the surface of a porous PE diaphragm and dried, the membrane is peeled off, and immersed in a 15-40wt% KOH solution at 80°C for more than three days for sufficient ion exchange, and then the membrane is taken out and the excess solution on the surface is wiped off to obtain a self-microporous polymer pore-filled ion solvated membrane.
[0018] The organic solvent is selected from dimethyl sulfoxide and N-methylpyrrolidone, and the mass concentration of the casting solution is controlled at 5-10 wt%.
[0019] The self-microporous polymer pore-filled ion solvation membrane of the present invention is used as a membrane electrode diaphragm material in hydrogen production in an alkaline water electrolyzer.
[0020] The alkaline water electrolyzer system includes a membrane electrode, bipolar plates arranged in sequence and a sealing element, wherein the membrane electrode further includes an electrode, a catalyst layer and an ion solvation membrane; the temperature test range is 40-80°C.
[0021] The present invention introduces an indole-2,3-dione structure and adopts a synthetic method of superacid-catalyzed hydroxyalkylation polymerization reaction, which effectively improves the chemical stability, thermal stability and mechanical stability of the polymer film; the self-microporous polymer has inherent micropores, which helps to promote the conduction of ions in the microporous channel, and also helps to transport water molecules in the channel, accelerating the hydrogen reduction reaction; the porous PE film is introduced as a base and support layer to enhance the mechanical stability of the polymer film. Using the self-microporous polymer containing the indole ketone structure and its ion solvation membrane and pore-filled ion solvation membrane as the diaphragm of AWE can effectively improve the electrolytic performance and service life of the electrolytic cell, promote the development of AWE, and promote the commercialization process.
[0022] Compared with the prior art, the beneficial effects of the present invention are as follows: The present invention selects indole-2,3-dione monomers and twisted rigid monomers as polymerization reaction monomers to carry out superacid catalyzed hydroxyalkylation polymerization reaction. The synthesized aromatic ether-free main chain can avoid polymer chemical degradation caused by ether bond rupture, thereby effectively improving the chemical stability, thermal stability and mechanical stability of the polymer film. The side group of indole ketone also has good stability under strong alkaline conditions, thereby effectively improving the chemical stability of the ion solvation membrane; the introduction of the twisted rigid monomer makes it impossible for the polymer chains to be densely stacked, forming an inherent microporous structure, thereby facilitating the rapid transmission of ions in the microporous channel.
[0023] Another innovation of the present invention is that, by further using a porous PE diaphragm as a substrate and a supporting layer, the problem of insufficient mechanical strength and toughness of the original homogeneous solvation membrane is solved, and the pore-filled ion solvation membrane has higher mechanical strength and longer service life. In short, using the self-microporous polymer based on indole-2,3-dione and its ion solvation membrane, and the pore-filled ion solvation membrane as a diaphragm in an alkaline water electrolyzer can improve the electrolytic performance of the electrolyzer, promote the development of alkaline water electrolyzers, and promote the commercialization process. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 Schematic diagram of the synthesis of the biphenyl-based indole-containing self-microporous polymer in Example 1.
[0025] Figure 2 This is the NMR image of the biphenyl-based self-microporous polymer containing indole structure in Example 1.
[0026] Figure 3 This is a graph showing the carbon dioxide adsorption-desorption curve of the biphenyl-based indolinone-containing self-microporous polymer in Example 1.
[0027] Figure 4 1 is a pore size distribution curve of the biphenyl-based indolinone-containing self-microporous polymer in Example 1.
[0028] Figure 5 3 is the stress-strain diagram of the biphenyl-based self-microporous polymer membrane containing indolinone structure in Example 1.
[0029] Figure 6 This is a thermogravimetric curve of the biphenyl-based self-microporous polymer containing an indolinone structure in Example 1.
[0030] Figure 7 3 is the EIS graph of the membrane electrode of the biphenyl-based indolinone structure-containing self-microporous ion solvation membrane in Example 1.
[0031] Figure 8 The water electrolysis performance of the biphenyl-based indolinone structure-containing self-microporous ion solvation membrane in Example 1 at 40°C.
[0032] Fig. 9 The electrolysis performance of the biphenyl-based indolinone-containing self-microporous ion solvation membrane in Example 1 at 60°C.
[0033] Fig.10 The electrolysis performance of the biphenyl-based indolinone-containing self-microporous ion solvation membrane in Example 1 at 80°C.
[0034] Fig.11 This is a schematic diagram of the synthesis of the self-microporous polymer containing indole structure based on 9,9-dimethylfluorene in Example 2.
[0035] Fig.12 This is the NMR image of the self-microporous polymer containing indole ketone structure based on 9,9-dimethylfluorene in Example 2.
[0036] Fig.13 This is a graph showing the carbon dioxide adsorption-desorption curve of the self-microporous polymer containing an indolone structure based on 9,9-dimethylfluorene in Example 2.
[0037] Fig.14 The electrolysis performance of the self-microporous ion solvation membrane containing indolone structure based on 9,9-dimethylfluorene in Example 2 at 80°C.
[0038] Fig.15 Schematic diagram of the synthesis of the self-microporous polymer containing indole structure based on spiro-(adamantane-2,9'-fluorene) in Example 3.
[0039] Fig.16 This is the NMR image of the self-microporous polymer containing indole ketone structure based on spiro-(adamantane-2,9'-fluorene) in Example 3.
[0040] Fig.173 is a graph showing the carbon dioxide adsorption-desorption curve of the self-microporous polymer containing an indolone structure based on spiro-(adamantane-2,9'-fluorene) in Example 3.
[0041] Fig.18 The electrolytic water performance of the self-microporous ion solvation membrane containing indolone structure based on spiro-(adamantane-2,9'-fluorene) in Example 3 at 80°C.
[0042] Fig.19 The electrolytic water performance of the self-microporous polymer containing indolone structure based on spiro-(adamantane-2,9'-fluorene) and its pore-filled ion solvation membrane at 80°C in Example 4. DETAILED DESCRIPTION
[0043] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.
[0044] In view of the problems that the key core component diaphragm has high surface resistance, serious gas crossover, poor electrolytic performance, insufficient mechanical strength and stability in the existing alkaline water electrolyzer membrane system, the present invention provides a self-microporous polymer based on indole-2,3-dione and its ion solvation membrane, a preparation method of pore-filled ion solvation membrane and alkaline water electrolyzer hydrogen production application. The present invention selects indole-2,3-dione monomer and twisted rigid monomer as polymerization reaction monomers to carry out superacid catalyzed hydroxyalkylation polymerization reaction, thereby effectively improving the chemical stability, thermal stability and mechanical stability of the polymer membrane. The side group of indole ketone also has good stability under strong alkaline conditions, thereby effectively improving the chemical stability of the ion solvation membrane. The introduction of twisted rigid monomers makes it impossible for the polymer chains to be tightly stacked, forming an inherent microporous structure, which helps to quickly transfer ions in the microporous channel, thereby improving the electrolytic performance. By using a porous PE diaphragm as a substrate and a supporting layer, the problem of insufficient mechanical strength and toughness of the original homogeneous ion solvation membrane is solved, and the pore-filled ion solvation membrane has higher mechanical strength and longer service life.
[0045] The embodiment of the present invention discloses a self-microporous polymer based on indole-2,3-dione and its ion solvation membrane, a preparation method of the pore-filled ion solvation membrane and its application in alkaline water electrolyzer for hydrogen production. The alkaline water electrolyzer hydrogen production application is that the ion solvation membrane and the pore-filled ion solvation membrane are used as membrane electrode diaphragms. The alkaline water electrolyzer system includes a membrane electrode, bipolar plates arranged in sequence and a sealing element, etc., wherein the membrane electrode includes an electrode, a catalyst layer, and an ion solvation membrane; the temperature test range is 40~80℃.
[0046] In order to further understand the present invention, the following detailed description is given of a self-microporous polymer based on indole-2,3-dione and its ion solvation membrane, a method for preparing the pore-filled ion solvation membrane and its application in hydrogen production in an alkaline water electrolyzer provided by the present invention in combination with the embodiments. The protection scope of the present invention is not limited by the following embodiments. Embodiment 1:
[0047] A method for preparing a biphenyl-based indolinone-containing self-microporous polymer and its ion solvation membrane, and its application in hydrogen production in an alkaline water electrolyzer.
[0048] 1. Weigh 2.313 g of biphenyl and 2.868 g of indole-2,3-dione and dissolve them in 15 mL of dichloromethane and 13.8 mL of trifluoroacetic acid. Add 10 mL of trifluoromethanesulfonic acid and react at room temperature for 8-20 hours. When the viscosity of the polymerization reaction system is relatively high, slowly pour the reaction solution into water to precipitate the polymer, then wash and dry it several times to obtain a microporous polymer main chain. Figure 1 This is a schematic diagram of the synthesis of the indolinone-containing self-microporous polymer provided in Example 1 of the present invention. Figure 2 The NMR image of the self-microporous polymer containing indolinone provided in Example 1 of the present invention: The 1H NMR spectrum successfully confirmed the successful synthesis of the chemical structure of the self-microporous polymer containing indolinone structure.
[0049] 2. Weigh 0.5 g of a self-microporous polymer containing an indolinone structure, dissolve it in 10 mL of N-methylpyrrolidone, stir, and centrifuge to obtain a transparent 5 wt% polymer solution. Cast and dry the polymer solution, peel off the membrane, immerse it in a 30 wt% KOH solution at 80 °C for more than three days for sufficient ion exchange, then take out the membrane and wipe off the excess solution on the surface to obtain a self-microporous ion solvated membrane.
[0050] 3. Dry the prepared self-microporous polymer containing indole structure under vacuum for 24 hours. Weigh about 0.1 g into a test glass tube and perform BET carbon dioxide adsorption and desorption test at 273K. Figure 3 This is a graph showing the carbon dioxide adsorption and desorption curve of the self-microporous polymer containing an indolinone structure provided in Example 1 of the present invention. After DFT analysis, the pore size distribution of the self-microporous polymer containing an indolinone structure was obtained. Figure 4 This is a pore size distribution diagram of the self-microporous polymer containing indolinone structure provided in Example 1 of the present invention.
[0051] 4. Cut the self-contained microporous polymer membrane containing indole structure into 1 cm × 4 cm size and place it in DMA850 dynamic mechanical analyzer for mechanical property testing. Figure 5The stress-strain diagram of the self-microporous polymer membrane containing indolinone structure provided in Example 1 of the present invention: the prepared self-microporous polymer membrane containing indolinone structure has good mechanical properties, and the tensile strength can reach 45 MPa.
[0052] 5. Weigh 5 mg of the self-microporous polymer containing indolinone structure, place it in TGA Q5000, and conduct thermal stability test at a heating rate of 10°C / min from 100°C to 800°C in a nitrogen atmosphere. Figure 6 Thermogravimetric curve of the self-microporous polymer containing indolinone structure provided in Example 1 of the present invention: the weight loss below 400°C is the removal of free water and bound water in the polymer, and it is basically stable below 400°C, indicating that the polymer has good thermal stability and can meet the use requirements of temperature conditions.
[0053] 6. The self-contained microporous ion solvation membrane containing indole ketone structure and the commercial catalyst integrated electrode were assembled into a membrane electrode MEA, connected to the electrochemical workstation Bio-Logic BCS-815, and the EIS test was performed using the two-electrode method. The frequency was 100mHz to 10KHz, the current was 150mA, and the amplitude was 50mA. Figure 7 The EIS graph of the membrane electrode of the self-microporous ion solvation membrane containing indolinone structure provided in Example 1 of the present invention: According to the equivalent circuit calculation, the charge transfer resistance of the self-microporous ion solvation membrane MEA containing indolinone structure is only 0.51Ω cm 2 This indicates that a good material transfer channel is constructed in the self-microporous ion solvation membrane MEA containing indolinone structure, and ions can be quickly transferred from the ion channels in the membrane, so the material transfer resistance is significantly reduced.
[0054] 7. The MEA prepared in Example 1 was assembled into an alkaline water electrolyzer single cell, connected to a LANHE battery teststation, and an alkaline water electrolyzer hydrogen production single cell test was performed. The battery temperature was 40°C, 60°C, and 80°C. The positive electrode electrolyte speed was 100rpm, and the negative electrode electrolyte speed was 50rpm. Figure 8 The electrolytic performance of the membrane electrode containing the self-microporous ion solvation membrane containing indolinone structure provided in Example 1 of the present invention at 40°C. Fig. 9 The electrolytic performance of the membrane electrode containing the self-microporous ion solvation membrane containing indolinone structure provided in Example 1 of the present invention at 60°C. Fig.10 The electrolytic performance of the membrane electrode of the self-microporous ion solvation membrane containing indolinone structure provided in Example 1 of the present invention at 80°C: high electrolytic performance is achieved, and the current density is 1.74 A cm at 2V. -2 . Embodiment 2:
[0055] A preparation method of an indolinone-containing self-microporous polymer and its ion solvation membrane based on 9,9-dimethylfluorene, and its application in hydrogen production in an alkaline water electrolyzer.
[0056] 1. Weigh 1.942 g 9,9-dimethylfluorene and 1.932 g indole-2,3-dione and dissolve them in 10 mL dichloromethane and 9.2 mL trifluoroacetic acid, add 4.6 mL trifluoromethanesulfonic acid, and react at room temperature for 0.5-2 hours. When the viscosity of the polymerization reaction system is relatively high, slowly pour the reaction solution into water to precipitate the polymer, then wash and dry it several times to obtain a microporous polymer main chain. Fig.11 Schematic diagram of the synthesis of the indolinone-containing self-microporous polymer provided in Example 2 of the present invention. Fig.12 The NMR image of the self-microporous polymer containing indolinone provided in Example 2 of the present invention: The 1H NMR spectrum successfully confirmed the successful synthesis of the chemical structure of the self-microporous polymer containing indolinone structure.
[0057] 2. Repeat steps 2-7 of Example 1. Fig.13 This is a graph showing the carbon dioxide adsorption-desorption curve of the self-microporous polymer containing an indolinone structure provided in Example 2 of the present invention. Fig.14 The electrolytic performance of the membrane electrode containing the self-microporous ion solvation membrane containing indolinone structure provided in Example 2 of the present invention at 80°C. Embodiment 3:
[0058] A preparation method of an indolinone-containing self-microporous polymer and an ion solvation membrane based on spiro-(adamantane-2,9'-fluorene) and an application thereof in hydrogen production in an alkaline water electrolyzer.
[0059] 1. Weigh 1.43 g of spiro-(adamantane-2,9'-fluorene) and 0.89 g of indole-2,3-dione and dissolve them in 10 mL of dichloromethane and 4.6 mL of trifluoroacetic acid, add 2.3 mL of trifluoromethanesulfonic acid, and react at room temperature for 0.5-2 hours. When the viscosity of the polymerization reaction system is relatively high, slowly pour the reaction solution into water to precipitate the polymer, then wash it several times and dry it to obtain a microporous polymer main chain. Fig.15 This is a schematic diagram of the synthesis of the indolinone-containing self-microporous polymer provided in Example 1 of the present invention. Fig.16 The NMR image of the self-microporous polymer containing indolinone provided in Example 1 of the present invention: The 1H NMR spectrum successfully confirmed the successful synthesis of the chemical structure of the self-microporous polymer containing indolinone structure.
[0060] 2. Repeat steps 2-7 of Example 1. Fig.17 This is a graph showing the carbon dioxide adsorption-desorption curve of the self-microporous polymer containing an indolinone structure provided in Example 2 of the present invention. Fig.18The electrolytic performance of the membrane electrode containing the self-microporous ion solvation membrane containing indolinone structure provided in Example 3 of the present invention at 80°C. Embodiment 4:
[0061] A method for preparing a self-microporous polymer containing indolinone based on spiro-(adamantane-2,9'-fluorene) and an ion solvation membrane filled with the pores thereof, and an application thereof in hydrogen production in an alkaline water electrolyzer.
[0062] 1. Place a porous PE membrane on a flat glass plate, drip the polymer solution prepared in Example 3 evenly on the porous PE membrane, and place it on a heating plate to heat until the solvent evaporates completely. Peel off the membrane, immerse it in a 15-40wt% KOH solution at 80°C for more than three days to perform sufficient ion exchange, then take out the membrane and wipe off the excess solution on the surface to obtain a pore-filled microporous ion solvated membrane.
[0063] 2. Repeat steps 3-7 of Example 1.
[0064] Fig.19 The electrolytic performance of the membrane electrode containing the self-microporous ion solvation membrane containing indolinone structure provided in Example 4 of the present invention at 80°C.
[0065] As can be seen from the above examples, the self-microporous polymer containing an indolinone structure having a structure of formula I provided by the present invention is a self-microporous polymer containing an indolinone structure obtained by first reacting a twisted rigid monomer with indole-2,3-dione through superacid catalyzed hydroxyalkylation. The polymer is then dissolved in an organic solvent to prepare an ion solvation membrane and a pore-filling ion solvation membrane used in an alkaline water electrolyzer.
[0066] The above embodiments are only used to help understand the method and core idea of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
[0067] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A self-microporous polymer based on indole-2,3-dione, characterized in that Its general structural formula is shown in the following formula I: ; A is selected from the following groups: ; * indicates the connection location; n represents the number of repeating units, i.e., the degree of polymerization, 100≤n≤1000.
2. The method for preparing the self-microporous polymer according to claim 1, characterized in that The steps include: Dissolving the twisted rigid monomer and indole-2,3-dione in dichloromethane and trifluoroacetic acid, adding trifluoromethanesulfonic acid, and reacting at room temperature for 0.5-24 hours; after the reaction, pouring the reaction solution into water to precipitate the polymer, washing and drying, to obtain a self-microporous polymer based on indole-2,3-dione; The torsionally rigid monomer is selected from the compounds of the following structures: 。 3. The preparation method according to claim 2, characterized in that: The molar ratio of the twisted rigid monomer to indole-2,3-dione is 1:1; the ratio of the total molar amount of the twisted rigid monomer and indole-2,3-dione to the molar amount of trifluoromethanesulfonic acid is 1:(1-10).
4. A method for preparing a self-microporous ion solvation membrane using the self-microporous polymer according to claim 1, characterized in that The steps include: The indole-2,3-dione-based self-microporous polymer is dissolved in an organic solvent to obtain a casting solution; the casting solution is used to cast a film and dry it, the film is peeled off, and immersed in a 15-40wt% KOH solution at 80°C for more than three days for sufficient ion exchange, and then the film is taken out and the excess solution on the surface is wiped off, so as to obtain a self-microporous ion solvated membrane.
5. The method according to claim 4, characterized in that: The organic solvent is selected from dimethyl sulfoxide and N-methylpyrrolidone, and the mass concentration of the casting solution is controlled at 5-10 wt%.
6. The self-microporous ion solvation membrane prepared according to claim 4 is used as a membrane electrode diaphragm material in hydrogen production in an alkaline water electrolyzer.
7. A method for filling the ion solvation membrane with the self-microporous polymer pores according to claim 1, characterized in that The steps include: The indole-2,3-dione-based self-microporous polymer is dissolved in an organic solvent to obtain a casting solution; the casting solution is cast on the surface of a porous PE diaphragm and dried, the membrane is peeled off, and immersed in a 15-40wt% KOH solution at 80°C for more than three days for sufficient ion exchange, and then the membrane is taken out and the excess solution on the surface is wiped off to obtain a self-microporous polymer pore-filled ion solvated membrane.
8. The method according to claim 7, characterized in that: The organic solvent is selected from dimethyl sulfoxide and N-methylpyrrolidone, and the mass concentration of the casting solution is controlled at 5-10 wt%.
9. The self-microporous polymer pore-filled ion solvation membrane prepared in claim 7 is used as a membrane electrode diaphragm material in hydrogen production in an alkaline water electrolyzer.
Citation Information
Patent Citations
A long-branched chain double-comb-shaped polyarylindole anion exchange membrane and a preparation method thereof
CN109119662A