Degradable plastic master batch material containing sand and preparation method thereof
By combining sand and polyolefin resin in degradable plastic materials, the problem of poor compatibility between sand and polymer-based is solved, and the material is improved Mechanical properties and weather resistance achieve reduced manufacturing costs and improved biodegradability, and are suitable for a variety of environmentally friendly and biodegradable products.
Patent Information
- Application Number
- CN202411546728.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-01
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-11-01
AI Technical Summary
Existing degradable plastic materials produce toxic gases during combustion, contaminate soil, and have high manufacturing costs. The poor compatibility between sand and polymer matrix leads to insufficient aging resistance and mechanical properties of the material, making it difficult to balance the degradation speed and mechanical strength. .
Sand is used as the main inorganic component, combined with polyolefins at different softening points as polymer resin components, and combined with modified glass fibers and vinyl acetate-acrylic-maleic anhydride terpolymer to improve the compatibility of sand and polymer-based , improve the mechanical properties and weather resistance of the material.
It significantly reduces the manufacturing cost of materials, improves mechanical properties and biodegradability, ensures the water resistance and aging resistance of the materials, and can be used to produce environmentally friendly and degradable products, such as seedling pots and corrugated cardboard, and the degradation rate is moderate. Influence mechanical strength.
Smart Images

Figure CN119039707A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of environmentally friendly materials, and particularly relates to a sand-containing degradable plastic masterbatch material and a preparation method thereof. Background Art
[0002] Biodegradable plastics are currently an important material for solving environmental problems. Polylactic acid (PLA) material is a new type of polymer material that is currently widely used in industrial applications. China is vigorously promoting the use of biodegradable plastic PLA and its improved products to complete the green transformation of various industries. The treatment of PLA products after use requires a lot of energy when burned, and toxic and harmful gases are produced during the combustion process. What's more serious is that the particles after burning are buried in the soil, which will pollute and poison the soil and cause irreversible effects. It is not a qualified environmentally friendly material. In addition, the expensive manufacturing cost of PLA is several times that of other plastics.
[0003] PMU (Polymer-Metal Hybrid Unit) polymer materials can not only effectively reduce the dependence on traditional plastics, but also help improve the mechanical strength and anti-aging properties of packaging materials. Compared with traditional plastics, PMU materials have better performance in terms of temperature resistance, water resistance, and oil resistance, which enables them to better ensure the quality and safety of products when packaging liquid products such as synthetic gasoline. Biodegradability is a highlight of PMU materials. According to relevant research, PMU materials can be completely degraded within a few months under specific environmental conditions. This feature makes it have broad application prospects in the packaging industry.
[0004] The inventor's previous patent CN110527191A discloses an inorganic degradable plastic masterbatch, which contains the following components: 56-72% by mass of calcium carbonate ore powder; 3-10% by mass of polyethylene; 8-30% by mass of polypropylene; 2-5% by mass of glass fiber; and 3-5% by mass of additives; the proportion of calcium carbonate ore powder of different particle sizes in the above 56-72% by mass of calcium carbonate ore powder is: 230 mesh 5-15% particle diameter controlled at 65-60 microns; 250 mesh 5-15% particle diameter controlled at 60-55 microns; 300 mesh 5-15% particle diameter controlled at 55-50 microns; 400 mesh 20-40% particle diameter controlled at 50-35 microns; 800 mesh 10-45% particle diameter controlled at 20-10 microns; 1200 mesh 10-45% The particle diameter is controlled at 10-5 microns; among them, the overall average particle size of calcium carbonate powder must be between 20 microns and 45 microns. The material has good mechanical properties and biodegradability. However, the use of calcium carbonate powder requires strict control of the particle size of calcium carbonate powder to achieve suitable performance, and the manufacturing process is complicated and costly. Sand and gravel are widely available, cheap and easy-to-obtain materials. If sand and gravel can be used to prepare plastic masterbatch and do not affect mechanical properties and biodegradability, the manufacturing cost of PMU materials will be greatly reduced. However, sand and polymer base have low affinity, and physical blending cannot solve the problem of interface compatibility, resulting in poor aging resistance and toughness of the resulting material, and defects such as weak points in mechanical properties.
[0005] CN113603938A discloses a starch-based degradable safety and environmentally friendly packaging box, which is composed of the following raw materials by weight: 40-50 parts of starch-based materials, 20-30 parts of polypropylene, 2-6 parts of polyolefin elastomers, 5-11 parts of glycerol, 25-35 parts of fillers, 0.5-1.5 parts of antioxidants, 5-10 parts of lignocellulose aerogels, and 10-20 parts of biochar. Wherein the filler can be sand and gravel powder, but the starch-based material belongs to incomplete biodegradable plastics, and the starch-based material will cause the entire material to become fragments after decomposition. These fragments are difficult to degrade and difficult to recycle and remove, and will damage the soil environment. Moreover, this type of material has poor high temperature and high humidity resistance and cannot be used as a material for long-term contact with hot water or high temperature and humidity environments.
[0006] CN118480229A discloses a flame-retardant polypropylene plastic fresh-keeping box with added sand and calcined shell powder, comprising the following raw materials by weight: 80-100 parts of polypropylene, 40-60 parts of modified calcined shell powder, 41-49 parts of silica sol, 40-50 parts of expanded perlite, 10-20 parts of sand-based composite aerogel, 5-10 parts of coupling agent, 2-3 parts of dispersant, 3-5 parts of plasticizer, and 0.01-0.03 parts of flame retardant; the modified calcined shell powder is prepared by pre-treatment. The shell powder is calcined at high temperature, mixed with a cerium source and an organic intercalation agent, and then subjected to hydrothermal treatment to obtain the aerogel; the pretreated shell powder is washed by the shell powder, ground into powder, sieved, and treated with an alkali agent; the sand-based composite aerogel is mixed with porous carbon-loaded sand and an antioxidant, added to cellulose nanofibers and melamine formaldehyde resin for cross-linking, and then freeze-dried; the porous carbon-loaded sand is washed and dried by the sand, then mixed with a carbon precursor and a connector, and subjected to high-temperature carbonization to obtain the aerogel. Although sand is used as the raw material for manufacturing safes, the sand needs to undergo a complicated preparation process to become a sand-based composite aerogel, and the manufacturing cost is still high, which is not suitable for large-scale industrial production.
[0007] CN102295793A discloses a highly filled oxidatively degradable polymer packaging material, which is formed by mixing and extruding the following components, wherein the components are measured by weight: 70-90 parts of inorganic fillers, 10-30 parts of polyolefin polymers, 0.01-0.2 parts of optical functional additives, 0.01-0.2 parts of thermal functional additives, 0.05-5 parts of coupling agents, and 0.01-5 parts of lubricants. Through the optical functional additives and thermal functional additives, the material is decomposed into fragments under the action of oxygen and sunlight, and further degraded into carbon dioxide and water. The content of inorganic fillers reaches more than 70%. However, the compatibility problem between sand and polymer matrix has not been solved.
[0008] In addition, the balance between the degradation rate and mechanical strength of such degradable materials is also a technical problem that needs to be solved. If the degradation rate is too fast, the material will quickly lose its mechanical strength; while increasing the mechanical strength will often reduce the degradability of the material. Therefore, the balance between the degradability and mechanical properties of such materials is also a problem that needs to be solved. Summary of the invention
[0009] In order to solve the above technical problems, the present invention provides a material with sand as the main inorganic component, polyolefins with different softening points as the polymer resin component, modified glass fiber and vinyl acetate-acrylic acid-maleic anhydride terpolymer, which solves the problem of poor compatibility between sand and polymer base, and significantly improves the mechanical properties and weather resistance of the material without affecting the degradability of the material. The preparation method of the present invention is simple, low in cost, and the raw materials are cheap and easy to obtain. The prepared masterbatch has excellent mechanical properties, biodegradability, water resistance and aging resistance. It can be used to produce various environmentally friendly degradable products such as seedling pots, corrugated cardboard, water pipes, etc. Specifically, the present invention provides the following technical solutions to achieve the above purpose.
[0010] A sand-containing degradable plastic masterbatch material comprises the following raw materials in parts by mass: 40-60 parts of sand powder, 6-10 parts of high-density polyethylene, 3-5 parts of low-density linear polyethylene, 22-28 parts of polypropylene, 5-8 parts of silica sol, 4-7 parts of coupling agent-modified glass fiber, 2-4 parts of ferrocene-modified glass fiber, and 3-7 parts of vinyl acetate-acrylic acid-maleic anhydride terpolymer; the coupling agent-modified glass fiber is obtained by modifying the glass fiber with a compounded coupling agent, the compounded coupling agent comprises coupling agent I and coupling agent II, the coupling agent I is selected from at least one of titanate coupling agent, aluminate coupling agent, and zirconate coupling agent, and the coupling agent II is selected from at least one of aminosilane coupling agent and epoxysilane coupling agent; the ferrocene-modified glass fiber is obtained by first coating the glass fiber with dopamine and then surface-modifying the glass fiber with ferrocene.
[0011] Further, the vinyl acetate-acrylic acid-maleic anhydride terpolymer is a terpolymer of vinyl acetate, acrylic acid and maleic anhydride in a mass ratio of 30-50:20-30:7-12. Further, the weight average molecular weight of the vinyl acetate-acrylic acid-maleic anhydride terpolymer is 20,000-30,000.
[0012] Furthermore, the vinyl acetate-acrylic acid-maleic anhydride terpolymer is prepared by a preparation method comprising the following steps: after water and an emulsifier are uniformly mixed to form an emulsion, monomers of vinyl acetate, acrylic acid, maleic anhydride and an initiator are added, the temperature is raised to an initiation temperature under an inert atmosphere for sufficient reaction, and after the reaction is completed, the obtained mixture is post-treated to obtain the vinyl acetate-acrylic acid-maleic anhydride terpolymer.
[0013] Further, the emulsifier is at least one of a nonionic surfactant and an anionic surfactant; preferably, the nonionic surfactant and the anionic surfactant are compounded in a mass ratio of 1-5:1-5, and the anionic surfactant and the nonionic surfactant are not particularly limited and are well known in the art, such as the anionic surfactant is SDS and the nonionic surfactant is Tween 80; the emulsifier accounts for 6-10wt% of the total mass of water and the emulsifier; the nitrogen atmosphere is at least one of nitrogen, argon and helium; the initiator is selected from at least one of ammonium persulfate, sodium persulfate and potassium persulfate, and the amount of the initiator is 0.5-1wt% of the total mass of the monomers. The initiation temperature is determined by the initiator used, such as for ammonium persulfate, the initiation temperature is 80-95°C, and the reaction time is 3-5h; the post-treatment is to add calcium chloride to break the emulsion, and the flocculants are filtered and then repeatedly washed with deionized water for 3-5 times, and dried to constant weight.
[0014] Furthermore, the size of the coupling agent modified glass fiber is a single fiber diameter of 5-8 μm and a length of 7-12 mm, and the size of the ferrocene modified glass fiber is a diameter of 2-4 μm and a length of 1-2 mm.
[0015] The coupling agent modified glass fiber is relatively long, which can better improve the compatibility of sand and polymer resin; the ferrocene modified glass fiber adopts short chopped fibers, and the ferrocene loaded therein acts as a degradation promoter, which can make the obtained material have a suitable degradation rate, so as to avoid the initial degradation and cause the mechanical strength to decrease, but make the material reach the purpose of being completely degradable.
[0016] Furthermore, the mass ratio of coupling agent I to coupling agent II is 1:2-3, and coupling agent II is preferably a compound of aminosilane coupling agent and epoxysilane coupling agent in a mass ratio of 1-3:1-3.
[0017] Further, the titanate coupling agent is selected from at least one of isopropyl dioleyl (dioctyl phosphate) titanate, isopropyl tri (dioctyl phosphate) titanate, tri (4-dodecylbenzenesulfonyl) isopropyl titanate, triisostearate isopropyl titanate, tetraisopropyl di (dioctyl phosphite) titanate, tri (dioctyl pyrophosphite) isopropyl titanate, tetraisopropyl titanate di (dilauryl phosphite), tri (diphenylpropane) -isopropyl titanate; the aluminate coupling agent is selected from distearoyloxy isopropyl aluminum The invention relates to a novel coupling agent for preparing the present invention. The invention relates to a coupling agent for preparing the present invention. The invention relates to a coupling agent for preparing the present invention. The invention relates to a coupling agent for preparing the present invention. The invention relates to a coupling agent for preparing the present invention. The invention relates to a coupling agent for preparing the present invention. The invention relates to a coupling agent for preparing the present invention. The invention relates to a coupling agent for preparing the present invention. The invention relates to a coupling agent for preparing the present invention.
[0018] The coupling agent modified glass fiber is prepared by a preparation method comprising the following steps: dispersing the surface cleaned glass fiber in an alcohol solvent, adding a compounded coupling agent, stirring and shaking the solution and heating it to 40-50° C. and keeping it warm, stirring and shaking for 1-3 hours, taking out the glass fiber and drying it to obtain the coupling agent modified glass fiber.
[0019] Furthermore, the alcohol solvent is selected from at least one of methanol, ethanol and isopropanol; and the amount of the compounded coupling agent is 5-10wt% of the surface cleaned glass fiber.
[0020] The ferrocene modified glass fiber is prepared by a preparation method comprising the following steps: (L1) adding the cleaned glass fiber to a dopamine buffer solution, stirring at room temperature for 20-30 hours, filtering, washing, and drying to obtain a dopamine-coated glass fiber; (L2) adding dopamine-coated glass fiber to dopamine buffer dispersed with ferrocene, stirring at room temperature for 20-30 hours, filtering, washing, and drying to obtain ferrocene-modified glass fiber.
[0021] Furthermore, in step (L1), the dopamine concentration in the dopamine buffer is 3-6 g / L; the ratio of the mass of the surface-cleaned glass fiber to the volume of the dopamine buffer is 1 g:10-20 mL; in step (L2), the dopamine concentration in the dopamine buffer dispersed with ferrocene is 1-2 g / L, and the ferrocene concentration is 1-3 g / L; the ratio of the mass of the dopamine-coated glass fiber to the volume of the dopamine buffer dispersed with ferrocene is 1 g:10-20 mL.
[0022] The dopamine buffer solution is prepared by preparing dopamine in the form of a 3-6 g / L dopamine aqueous solution, adjusting the pH value to 8-9 with Tris-HCl, and uniformly dispersing the solution.
[0023] The surface cleaning of glass fiber is well known in the art. Since the surface of commercially available glass fiber contains a wetting agent, this part of the wetting agent needs to be removed before modification. The specific method is to place the glass fiber in a muffle furnace and calcine it at 400-600° C. for 3-5 hours.
[0024] Furthermore, the mass ratio of the sum of sand powder and polymer (ie, the sum of high-density polyethylene, low-density linear polyethylene and polypropylene) is 1.2-1.5:1.
[0025] Furthermore, the high-density polyethylene has a crystallinity of 81-88% and a softening point of 125-135°C; the linear low-density polyethylene has a softening point of 110-115°C; and the polypropylene has a softening point of 140-155°C.
[0026] Furthermore, the sand powder is ground into 1000-1500 meshes. The present invention only needs to grind common sand and gravel into a specified particle size, does not require complex grading, has low cost and a wide range of sources.
[0027] Optionally, the sand-containing degradable plastic masterbatch material further comprises the following auxiliary agents in parts by weight: 0.5-1 part of lubricant, 0.1-0.3 part of antioxidant, and 0.3-0.5 part of plasticizer. The lubricant, antioxidant, and plasticizer are well known in the art, for example, the antioxidant is selected from antioxidant 1010 and antioxidant 168; the lubricant is selected from at least one of paraffin wax, polypropylene wax, and stearate; the plasticizer is selected from at least one of tributyl citrate, polyethylene glycol, dioctyl phthalate, and methyl acetyricinoleate.
[0028] The present invention also provides a method for preparing the above-mentioned sand-containing degradable plastic masterbatch material, comprising the following steps: (S1) grinding sand to obtain sand powder of suitable fineness, adding the sand powder, high-density polyethylene, low-density linear polyethylene polypropylene, silica sol, coupling agent modified glass fiber, ferrocene modified glass fiber, and vinyl acetate-acrylic acid-maleic anhydride terpolymer into a mixer, optionally, adding auxiliary materials, mixing evenly under ultrasonic vibration conditions and exhausting to obtain a precursor; (S2) The precursor is added into a mixing and melting device, extruded into strips at a temperature of 240-250° C., pelletized after water cooling, and dehydrated to obtain a sand-containing biodegradable plastic masterbatch material.
[0029] Furthermore, in step (S1), the ultrasonic vibration condition is a vibration frequency of 50-100 kHz, and the internal mixing and melting equipment is a single-screw extruder, a twin-screw extruder or a triple-screw extruder.
[0030] The present invention realizes the preparation of a degradable plastic material with excellent comprehensive performance by using sand as the main inorganic component and polyolefin as the resin component through the reasonable optimization and compatibility of the glass fiber modified by the coupling agent and the vinyl acetate-acrylic acid-maleic anhydride terpolymer, thereby improving the compatibility of the sand and the resin component, improving the mechanical properties of the material, and improving the tensile strength and elongation at break of the material, that is, achieving the effect of strengthening and toughening at the same time. Ferrocene-modified glass fiber not only improves the strength of the material, but also does not require the additional addition of photosensitizers or catalysts. Ferrocene with degradation-promoting activity is loaded on short chopped glass fibers, thereby ensuring the mechanical strength of the material for a long time and giving the material sufficient degradation performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is an optical microscope photograph of the sand-containing degradable plastic masterbatch material prepared in Example 1.
[0032] Figure 2 This is a physical photo of the sand-containing degradable plastic masterbatch material prepared in Example 1. DETAILED DESCRIPTION
[0033] High-density polyethylene is purchased from Yanshan Petrochemical, with a crystallinity of 82% and a softening point of 131°C; linear low-density polyethylene is purchased from Yanshan Petrochemical, with a softening point of 112°C; and polypropylene is purchased from Yanshan Petrochemical, with a softening point of 145°C.
[0034] Preparation Example 1 SDS: Tween 80 was used as a compound emulsifier, and the emulsion was stirred and prepared. The mass ratio of the compound emulsifier to water was 6:94. The monomers of vinyl acetate, acrylic acid and maleic anhydride were added in a mass ratio of 50:30:7, and then 1wt% of the total mass of the monomers was added as an initiator. The temperature was raised to 85°C under a nitrogen atmosphere, and the reaction was kept warm for 3 hours. After cooling to room temperature, CaCl2 was added to break the emulsion, and the flocculants were filtered and washed with deionized water for 3 times, and dried to constant weight to obtain vinyl acetate-acrylic acid-maleic anhydride terpolymer a. After testing, the weight average molecular weight of terpolymer a was about 28,000.
[0035] Preparation Example 2 The other conditions were the same as those in Preparation Example 1, except that the mass ratio of the monomers vinyl acetate, acrylic acid and maleic anhydride was 30:20:12, and vinyl acetate-acrylic acid-maleic anhydride terpolymer b was obtained. After testing, the weight average molecular weight of the terpolymer b was about 22,000.
[0036] Preparation Example 3 Long glass fiber (diameter 5 μm, length 10 mm) was placed in a muffle furnace and heated to 500°C for calcination for 3 hours to complete surface cleaning. 10 g of the long glass fiber with cleaned surface was dispersed in ethanol, and 0.5 g of a complex coupling agent was added. The complex coupling agent was a compound of isopropyl tri(dioctylphosphoyl) titanate, KH-540 and KH-560 in a mass ratio of 1:1:1. The dispersion was stirred and shaken, and the temperature was raised to 50°C. Stirring and shaking was maintained for 3 hours, and the glass fiber was taken out and dried to obtain a coupling agent modified glass fiber a.
[0037] Preparation Example 4 The other conditions were the same as those in Preparation Example 3, except that the long glass fiber (diameter 5 μm, length 10 mm) was replaced by the short glass fiber (diameter 3 μm, length 1 mm), and finally the coupling agent modified glass fiber b was obtained.
[0038] Preparation Example 5 The other conditions were the same as those in Preparation Example 3, except that the coupling agent was a compound of isopropyl tri(dioctylphosphoyl)titanate and KH-540 in a mass ratio of 1:2 to obtain coupling agent modified glass fiber c.
[0039] Preparation Example 6 The other conditions were the same as those in Preparation Example 3, except that the coupling agent was a compound of isopropyl tri(dioctylphosphoyl)titanate and KH-560 in a mass ratio of 1:2 to obtain coupling agent modified glass fiber d.
[0040] Preparation Example 7 (L1) Short glass fibers (3 μm in diameter and 1 mm in length) were placed in a muffle furnace and heated to 500°C for 3 h to complete surface cleaning. 1 g of the short glass fibers with cleaned surfaces was added to 20 mL of 5 g / L dopamine buffer (pH adjusted to 8.5 with tris-HCl), stirred at room temperature for 24 h, filtered, washed, and dried to obtain dopamine-coated glass fibers. (L2) Add 1 g of dopamine-coated glass fiber to a dopamine buffer solution dispersed with ferrocene (dopamine concentration 2 g / L, ferrocene concentration 2 g / L, pH = 8.5), stir at room temperature for 24 h, filter, wash, and dry to obtain ferrocene-modified glass fiber a.
[0041] Preparation Example 8 Other conditions and operations were the same as those in Preparation Example 7, except that the short glass fiber was replaced by a long glass fiber (8 μm in diameter and 6 mm in length), and finally ferrocene-modified glass fiber b was obtained.
[0042] Comparative Example Preparation Example 1 The other conditions were the same as those in Preparation Example 3, except that the coupling agent was only isopropyl tri(dioctylphosphoyloxy)titanate, that is, coupling agent II was not added, and finally coupling agent-modified glass fiber e was obtained.
[0043] Comparative Example Preparation Example 2 The other conditions were the same as those in Preparation Example 3, except that the coupling agent was a compound of KH-540 and KH-560 in a mass ratio of 1:1, that is, no coupling agent I was added, and finally a coupling agent-modified glass fiber f was obtained.
[0044] Comparative Example Preparation Example 3 The other conditions were the same as those in Preparation Example 7, except that in step (L2), ferrocene was replaced by an equal mass of nano-iron oxide (D50=20 nm), and the concentration of nano-iron oxide was 2 g / L, and finally iron oxide-modified glass fiber was obtained.
[0045] Example 1 (S1) grinding sand to obtain 1500 mesh sand powder by screening, adding 50 parts by mass of sand powder, 7 parts by mass of high-density polyethylene, 5 parts by mass of low-density linear polyethylene, 25 parts of polypropylene, 5 parts of silica sol, 5 parts of coupling agent modified glass fiber a obtained in Preparation Example 3, 2 parts of ferrocene modified glass fiber a obtained in Preparation Example 7, vinyl acetate-acrylic acid-maleic anhydride terpolymer a obtained in Preparation Example 1, and 0.5 parts of ferric stearate, 0.1 parts of antioxidant 1010, and 0.3 parts of plasticizer tributyl citrate into a mixer, mixing evenly under ultrasonic vibration conditions and exhausting, to obtain a precursor; (S2) The precursor is added into a three-screw extruder, extruded into strips at a temperature of 240-250° C., pelletized after water cooling, and dehydrated to obtain a sand-containing biodegradable plastic masterbatch material.
[0046] Figure 1 This is an optical microscope photo of the sand-containing degradable plastic masterbatch material obtained in Example 1. It can be seen that the sample contains fiber piles and blocky substances. Figure 2 This is a physical photo of the sand-containing degradable plastic masterbatch material prepared in Example 1.
[0047] Example 2 The other conditions are the same as those in Example 1, except that the coupling agent modified glass fiber a prepared in Preparation Example 3 is replaced by the coupling agent modified glass fiber b prepared in Preparation Example 4.
[0048] Example 3 The other conditions are the same as those in Example 1, except that the coupling agent modified glass fiber a prepared in Preparation Example 3 is replaced by the coupling agent modified glass fiber c prepared in Preparation Example 5.
[0049] Example 4 The other conditions are the same as those in Example 1, except that the coupling agent modified glass fiber a prepared in Preparation Example 3 is replaced by the coupling agent modified glass fiber d prepared in Preparation Example 6.
[0050] Example 5 The other conditions are the same as those in Example 1, except that the ferrocene-modified glass fiber a prepared in Preparation Example 7 is replaced by the ferrocene-modified glass fiber b prepared in Preparation Example 8.
[0051] Example 6 The other conditions were the same as those in Example 1, except that the terpolymer a in Preparation Example 1 was replaced by the terpolymer b prepared in Preparation Example 2.
[0052] Comparative Example 1 The other conditions are the same as those in Example 1, except that the coupling agent modified glass fiber a prepared in Preparation Example 3 is replaced by the coupling agent modified glass fiber e prepared in Comparative Preparation Example 1.
[0053] Comparative Example 2 The other conditions are the same as those in Example 1, except that the coupling agent modified glass fiber a prepared in Preparation Example 3 is replaced by the coupling agent modified glass fiber f prepared in Comparative Preparation Example 2.
[0054] Comparative Example 3 The other conditions are the same as those in Example 1, except that the ferrocene-modified glass fiber a prepared in Preparation Example 7 is replaced by the iron oxide-modified glass fiber prepared in Comparative Preparation Example 3.
[0055] Application Examples The sand-containing degradable plastic masterbatch materials of the above examples and comparative examples were subjected to the following performance tests, and the results are shown in Table 1.
[0056] The tensile strength was tested according to ASTM D638, the flexural strength was tested according to ASTM D790, and the degradation performance was tested according to ASTM D5511. The accelerated degradation conditions were to apply a fluorescent lamp with a power of 30W, an irradiation distance of 50cm, and a temperature of 25±3℃. Table 1 Masterbatch performance test
Claims
1. A sand-containing degradable plastic masterbatch material, characterized in that: The invention comprises the following raw materials in parts by mass: 40-60 parts of sand powder, 6-10 parts of high-density polyethylene, 3-5 parts of low-density linear polyethylene, 22-28 parts of polypropylene, 5-8 parts of silica sol, 4-7 parts of coupling agent modified glass fiber, 2-4 parts of ferrocene modified glass fiber, and 3-7 parts of vinyl acetate-acrylic acid-maleic anhydride terpolymer; the coupling agent modified glass fiber is obtained by modifying the glass fiber with a compound coupling agent, the compound coupling agent comprises coupling agent I and coupling agent II, the coupling agent I is selected from at least one of titanate coupling agent, aluminate coupling agent and zirconate coupling agent, and the coupling agent II is selected from at least one of aminosilane coupling agent and epoxysilane coupling agent; the ferrocene modified glass fiber is obtained by first coating the glass fiber with dopamine and then surface-modifying the glass fiber with ferrocene.
2. The sand-containing degradable plastic masterbatch material according to claim 1, characterized in that: The vinyl acetate-acrylic acid-maleic anhydride terpolymer is a terpolymer of monomers of vinyl acetate, acrylic acid and maleic anhydride in a mass ratio of 30-50:20-30:7-12; the weight average molecular weight of the vinyl acetate-acrylic acid-maleic anhydride terpolymer is 20000-30000.
3. The sand-containing degradable plastic masterbatch material according to claim 2, characterized in that: The vinyl acetate-acrylic acid-maleic anhydride terpolymer is prepared by a preparation method comprising the following steps: after water and an emulsifier are uniformly mixed to form an emulsion, monomers of vinyl acetate, acrylic acid, maleic anhydride and an initiator are added, the temperature is raised to an initiation temperature under an inert atmosphere to fully react, and after the reaction is completed, the obtained mixture is post-treated to obtain the vinyl acetate-acrylic acid-maleic anhydride terpolymer; The emulsifier is at least one of a nonionic surfactant and an anionic surfactant, and the nonionic surfactant and the anionic surfactant are compounded in a mass ratio of 1-5:1-5; the emulsifier accounts for 6-10wt% of the total mass of water and the emulsifier; the nitrogen atmosphere is at least one of nitrogen, argon and helium; the initiator is selected from at least one of ammonium persulfate, sodium persulfate and potassium persulfate, and the amount of the initiator is 0.5-1wt% of the total mass of the monomers; the initiation temperature is 80-95°C, and the reaction time is 3-5h; the post-treatment is adding calcium chloride to break the emulsion, and the flocculants are filtered and then repeatedly washed with deionized water for 3-5 times, and dried to constant weight.
4. The sand-containing degradable plastic masterbatch material according to claim 1, characterized in that: The size of the coupling agent modified glass fiber is 5-8 μm in diameter and 7-12 mm in length; the size of the ferrocene modified glass fiber is 2-4 μm in diameter and 1-2 mm in length.
5. The sand-containing degradable plastic masterbatch material according to claim 1, characterized in that: The mass ratio of coupling agent I to coupling agent II is 1:2-3.
6. The sand-containing degradable plastic masterbatch material according to claim 1, characterized in that: The titanate coupling agent is selected from at least one of isopropyl dioleyl (dioctyl phosphate) titanate, isopropyl tri (dioctyl phosphate) titanate, tri (4-dodecylbenzenesulfonyl) isopropyl titanate, triisostearate isopropyl titanate, tetraisopropyl di (dioctyl phosphite) titanate, tri (dioctyl pyrophosphite) isopropyl titanate, tetraisopropyl titanate di (dilauryl phosphite), tri (diphenylpropane) -isopropyl titanate; the aluminate coupling agent is selected from distearoyloxy isopropyl aluminate, At least one of isopropoxy distearate acyloxyaluminate, triisopropoxy aluminum, and liquid aluminate coupling agents; the zirconate coupling agent is selected from at least one of tetrabutyl zirconate, tetraisopropyl zirconate, neoalkoxy tris (p-aminophenoxy) zirconate, tetrakis (triethanolamine) zirconate, and alkoxy tris (vinyl-ethoxy) zirconate; the aminosilane coupling agent is selected from at least one of KH-540 and KH-550; the epoxysilane coupling agent is selected from at least one of KH-560, KH-561, and KH-563.
7. The sand-containing degradable plastic masterbatch material according to claim 1, characterized in that: The coupling agent modified glass fiber is prepared by a preparation method comprising the following steps: dispersing the surface cleaned glass fiber in an alcohol solvent, adding a compounded coupling agent, stirring and shaking the solution and heating it to 40-50° C. and keeping it warm, stirring and shaking for 1-3 hours, taking out the glass fiber and drying it to obtain the coupling agent modified glass fiber; The alcohol solvent is selected from at least one of methanol, ethanol and isopropanol; the amount of the compounded coupling agent is 5-10wt% of the surface cleaned glass fiber.
8. The sand-containing degradable plastic masterbatch material according to claim 1, characterized in that: The ferrocene modified glass fiber is prepared by a preparation method comprising the following steps: (L1) adding the cleaned glass fiber to a dopamine buffer solution, stirring at room temperature for 20-30 hours, filtering, washing, and drying to obtain a dopamine-coated glass fiber; (L2) adding the dopamine-coated glass fiber to a dopamine buffer solution dispersed with ferrocene, stirring at room temperature for 20-30 hours, filtering, washing, and drying to obtain the ferrocene-modified glass fiber; In step (L1), the dopamine concentration in the dopamine buffer is 3-6 g / L; the ratio of the mass of the surface-cleaned glass fiber to the volume of the dopamine buffer is 1 g:10-20 mL; in step (L2), the dopamine concentration in the dopamine buffer dispersed with ferrocene is 1-2 g / L, and the ferrocene concentration is 1-3 g / L; the ratio of the mass of the dopamine-coated glass fiber to the volume of the dopamine buffer dispersed with ferrocene is 1 g:10-20 mL; The dopamine buffer solution is prepared by preparing dopamine in the form of a 3-6 g / L dopamine aqueous solution, adjusting the pH value to 8-9 with Tris-HCl, and uniformly dispersing the solution.
9. The sand-containing degradable plastic masterbatch material according to claim 1, characterized in that: The mass ratio of the sum of sand powder and polymer is 1.2-1.5:1, and the sum of polymer is the sum of high-density polyethylene, low-density linear polyethylene and polypropylene; and / or The high-density polyethylene has a crystallinity of 81-88% and a softening point of 125-135°C; the linear low-density polyethylene has a softening point of 110-115°C; and the polypropylene has a softening point of 140-155°C. The sand powder is ground into 1000-1500 meshes.
10. The method for preparing the sand-containing degradable plastic masterbatch material according to any one of claims 1 to 9, characterized in that: The following steps are involved: (S1) grinding sand to obtain sand powder, adding the sand powder, high-density polyethylene, low-density linear polyethylene, polypropylene, silica sol, coupling agent-modified glass fiber, ferrocene-modified glass fiber, and vinyl acetate-acrylic acid-maleic anhydride terpolymer into a mixer, optionally, adding auxiliary materials, mixing evenly under ultrasonic vibration conditions and exhausting to obtain a precursor; (S2) The precursor is added into a mixing and melting device, extruded into strips at a temperature of 240-250° C., pelletized after water cooling, and dehydrated to obtain a sand-containing biodegradable plastic masterbatch material.
Citation Information
Patent Citations
preparation method and application of acrylate wood-plastic composite compatibilization modifier
CN103146049A
Preparation method of dopamine-modified glass fiber-epoxy resin composite material
CN107226997A
Polypropylene composite material with high heat conductivity
CN107868337A
Flame-retardant continuous long glass fiber reinforced PP material used for wall switches, and preparation method thereof
CN108276664A
Corrosion-resistant impermeable membrane
CN108342010A
Cited By
Method for amplifying specific surface area of autotrophic nitrogen removal filler
CN120698604A