Modified polytetrafluoroethylene bearing material, manufacturing method and metal plastic sliding bearing
Through the composite materials of polytetrafluoroethylene, polyphenyl ester, modified wollastonite mineral fiber and hexagonal boron nitride, the problems of pure polytetrafluoroethylene materials are solved under high loads and poor mechanical properties are achieved. High wear resistance, high load and low cost modified PTFE bearing materials for high performance bearing applications.
Patent Information
- Application Number
- CN202411286314.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Pure polytetrafluoroethylene materials are prone to cold flow under high loads, have poor mechanical properties, insufficient wear resistance, and the existing modified filler materials have poor performance and high cost, which limits their application.
The modified polytetrafluoroethylene bearing material is prepared by mechanical blending, cold pressing preforming and vacuum sintering processes. In combination with metal plastic sliding bearings.
It significantly improves the friction and wear performance, mechanical properties and wear resistance of bearing materials, reduces production costs, and the product surface is white and smooth, improving aesthetics and economic benefits.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of modified manufacturing of polymer composite materials, and in particular relates to a modified polytetrafluoroethylene bearing material, a manufacturing method and a metal plastic sliding bearing. Background Art
[0002] Polytetrafluoroethylene (PTFE) is a polymer material with high stability and unique properties. Since the mutual attraction between PTFE macromolecules is small and the surface attraction to other molecules is also small, its friction coefficient is very small, and the static friction coefficient can reach 0.04, which is the smallest friction coefficient among known practical sliding materials and has abnormal lubrication properties. However, pure PTFE material also has many disadvantages. For example, poor mechanical strength, low hardness, poor creep resistance, and easy cold flow. There are also disadvantages and shortcomings such as large linear expansion coefficient, poor thermal conductivity, and poor wear resistance. For example, the PV value as a bearing material is small.
[0003] Therefore, pure PTFE has poor mechanical properties and is prone to "cold flow" under heavy loads, resulting in large viscous deformation and high wear rate. Due to poor creep resistance, the dimensional stability of bearing products is poor. These defects limit the application of PTFE materials to a certain extent. In order to improve the mechanical properties and wear resistance of PTFE materials, filler materials are used to modify them. On the basis of maintaining the excellent properties of PTFE materials, the comprehensive characteristics of composite materials are used to make up for their own shortcomings and improve the strength, rigidity, dimensional stability and wear resistance of composite materials.
[0004] Polymer bearing materials should have low friction coefficient and high wear resistance. Due to high load, bearing materials should have high load capacity, good wear resistance and self-lubrication, sufficient fatigue strength, good running-in and corrosion resistance. Good vibration and impact load resistance, thick wear-resistant layer to bring good noise elimination characteristics, to adapt to a wide range of matching clearance.
[0005] The fillers used to fill and modify PTFE are divided into inorganic fillers, organic fillers and fiber-reinforced fillers. Traditional modification methods mostly use inorganic fillers and fiber-reinforced fillers such as carbon fiber, glass fiber, graphite, and molybdenum disulfide to fill and modify PTFE in PTFE resin. These fillers either have unsatisfactory wear resistance, large friction coefficient, or poor mechanical properties. For example, glass fiber improves the hardness and wear resistance of PTFE composite materials, but increases the friction coefficient of the material and damages the wear parts. Although adding graphite or molybdenum disulfide anti-friction fillers can reduce the friction coefficient, it will make the product color black and reduce the mechanical properties. Carbon fiber can increase the tensile strength and compressive strength of PTFE composite materials, but it will reduce the impact strength. Therefore, for the blending and filling modification of PTFE bearing materials, it is necessary to select suitable filling materials for ternary or multi-component composite synergistic modification in order to obtain high-performance polymer bearing materials. In addition, the existing widely used modified PTFE filling materials not only have poor performance, but also have very high costs. Summary of the invention
[0006] The present invention provides a modified polytetrafluoroethylene bearing material, a manufacturing method and a metal plastic sliding bearing to solve the above-mentioned technical problems, and specifically adopts the following technical solutions: A modified polytetrafluoroethylene bearing material, comprising polytetrafluoroethylene, polyphenyl ester, modified wollastonite mineral fiber and hexagonal boron nitride; The weight percentages of the various components are as follows: The polytetrafluoroethylene powder accounts for 57-83%, the polyphenyl ester powder accounts for 10-20%, the modified wollastonite mineral fiber accounts for 5-15%, and the hexagonal boron nitride particles account for 2-8%.
[0007] Furthermore, the polytetrafluoroethylene powder is 65-75%, the polyphenyl ester powder is 13-17%, the modified wollastonite mineral fiber is 8-12%, and the hexagonal boron nitride particles are 3-7%.
[0008] Furthermore, the particle size of the polytetrafluoroethylene powder is 40-60 μm, the particle size of the polyphenyl ester powder is 30-40 μm, the particle size of the modified wollastonite mineral fiber is 7-10 μm, the aspect ratio is 15:1, and the particle size of the hexagonal boron nitride is 1-5 μm.
[0009] Furthermore, the particle size of the polytetrafluoroethylene powder is 30-70 μm, the particle size of the polyphenyl ester powder is 30-40 μm, the particle size of the modified wollastonite mineral fiber is 7-10 μm, the aspect ratio is 15:1, and the particle size of the hexagonal boron nitride is 1-5 μm.
[0010] A method for manufacturing a modified polytetrafluoroethylene bearing material comprises the following steps: (1) Mix the above polymer materials and filler materials together in a certain proportion, mix them thoroughly and evenly by mechanical blending, and dry the mixed powder; (2) Place the prepared copper wire pad into the mold, spread the mixed and dried powder on the copper wire pad, and place it on a hydraulic press for cold pressing and preforming; (3) The preformed and pressed blank is placed in a vacuum sintering furnace for heating and sintering, and then taken out of the furnace after cooling.
[0011] Furthermore, the drying process was carried out at a temperature of 90° for 6 hours.
[0012] Furthermore, the cold press preforming condition is a pressure of 50-70 MPa / cm 2 , maintain pressure for 3-5 minutes.
[0013] Furthermore, the heating and sintering conditions are: a sintering temperature of 360° C.-395° C. and a constant temperature of 40 min-55 min.
[0014] Furthermore, after heating and sintering, the sintered product is cooled to less than 80°C before being taken out of the furnace.
[0015] Furthermore, the prepared modified polytetrafluoroethylene bearing tile surface is brazed to the metal matrix steel tile base to obtain a metal-plastic sliding bearing composited with the modified polytetrafluoroethylene bearing material tile surface and the metal matrix steel tile base.
[0016] The addition of polyphenylene ester significantly improves the friction and wear properties of bearing materials. Polyphenylene ester can be blended with PTFE in any proportion. The blended material can not only maintain the advantages of the two polymers such as heat resistance, wear resistance, self-lubrication, etc., but also complement each other in performance, overcoming the easy creep of PTFE and the brittleness of polyphenylene ester. The filling of polyphenylene ester improves the tribological properties of PTFE composite materials.
[0017] The present invention selects modified wollastonite mineral fiber to replace carbon fiber or glass fiber, and adds hexagonal boron nitride particles to replace graphite and molybdenum disulfide, thereby achieving better lubrication efficiency. The modified wollastonite mineral fiber and the hexagonal boron nitride particles synergistically modify the PTFE material. The modified wollastonite mineral fiber can significantly improve the mechanical and tribological properties of the matrix due to its high aspect ratio. Compared with pure PTFE material, the friction coefficient of the filled modified wollastonite mineral fiber is increased. Inorganic particle hexagonal boron nitride is a solid lubricant that can reduce the friction coefficient of PTFE composite materials and improve the self-lubricating properties of PTFE composite materials.
[0018] In summary, the modified polytetrafluoroethylene bearing material, manufacturing method and metal-plastic sliding bearing provided by the present invention use polyphenyl ester, modified wollastonite mineral fiber and hexagonal boron nitride to synergistically modify the PTFE bearing material, which makes up for the shortcomings of the prior art and provides a polytetrafluoroethylene bearing material and metal-plastic sliding bearing with high wear resistance, high load, high strength and good self-lubrication.
[0019] Moreover, after the existing filling materials replace the original carbon fiber, graphite or molybdenum disulfide, the surface of the product becomes white and smooth, which improves the defect of the original black surface color of the product and greatly improves the aesthetics of the product.
[0020] At the same time, the modified polytetrafluoroethylene bearing material of the present application greatly reduces the production cost by selecting low-priced modified wollastonite mineral fiber instead of carbon fiber. Carbon fiber is expensive, generally 100-200 yuan / kg depending on performance, while modified wollastonite mineral fiber is cheap, generally not exceeding 10 yuan / kg. Moreover, modified wollastonite mineral fiber has excellent performance as a filling material. Therefore, the modified polytetrafluoroethylene bearing material of the present application has low cost and excellent performance, achieves energy saving and efficiency improvement to a great extent, and significantly improves economic benefits and market competitiveness. DETAILED DESCRIPTION
[0021] The embodiments of the present application are described in detail below. The embodiments are exemplary and are intended to be used to explain the present application, but should not be construed as limiting the present application.
[0022] Polyparahydroxybenzoate, commonly known as polyphenylene ester (POB), is a high-temperature resistant special engineering plastic, light yellow to brownish yellow powder. POB has excellent performance, radiation resistance, and resistance to all organic solvents. The decomposition temperature is as high as 530°C, and it can be used for a long time at 300°C. It exhibits non-viscous flow like metal at high temperatures, has high compression strength, good creep resistance, and high ultimate PV value. Its crystals are flaky, similar to solid lubricants such as graphite and molybdenum disulfide. It has good self-lubricity and wear resistance. Compared with polymer materials such as PTFE under the same conditions, its wear is very small. These characteristics make it a lubricating filler with excellent performance. After filling PTFE resin material with POB, the obtained composite material has the advantages of good wear resistance and high PV value, but the mechanical properties are reduced. Multi-composite modified PTFE should be considered to improve its specific properties.
[0023] Modified wollastonite mineral fiber (MWF) is a calcium-containing metasilicate mineral. It has the characteristics of chemical corrosion resistance, good thermal stability and dimensional stability, excellent mechanical properties and electrical properties. At the same time, it is non-toxic and tasteless, safe and environmentally friendly, cheap and easy to obtain, and much cheaper than carbon fiber. But the performance is comparable to that of carbon fiber. Because it has needle-shaped and fibrous crystal forms, it has a series of excellent characteristics such as high aspect ratio and high activity, and has good compatibility with resin. It also has better load-bearing capacity and wear resistance. It is used as a modified reinforcing filler for polymer composite materials, which can significantly improve the mechanical and tribological properties of polymer composites. Single MWF fiber modified PTFE can increase the compression strength and reduce wear.
[0024] Hexagonal boron nitride (H-BN) particles have a layered structure similar to graphite and are known as white graphite. H-BN has good thermal and chemical stability, good electrical insulation, thermal conductivity, impact resistance and mechanical processing performance, outstanding wear resistance and lubricity, and is a lubricant for high temperature environments.
[0025] The invention discloses a modified polytetrafluoroethylene bearing material, which consists of polytetrafluoroethylene (PTFE), polyphenylene ester (POB), modified wollastonite mineral fiber (MWF) and hexagonal boron nitride (H-BN).
[0026] The weight percentages of the various components are as follows: PTFE powder is 57-83%, POB powder is 10-20%, MWF fiber is 5-15%, and H-BN particles are 2-8%.
[0027] Preferably, PTFE powder is 65-75%, POB is 13-17%, MWF fiber is 8-12%, and H-BN particles are 3-7%.
[0028] The particle size of the PTFE powder is 20-70 μm, the particle size of the POB powder is 20-50 μm, the particle size of the MWF fiber is 4-13 μm, the aspect ratio is 15:1, and the particle size of the hexagonal boron nitride is 1-5 μm.
[0029] Preferably, the particle size of the PTFE powder is 40-60 μm, the particle size of the POB powder is 30-40 μm, the particle size of the MWF fiber is 7-10 μm, the aspect ratio is 15:1, and the particle size of the hexagonal boron nitride is 1-5 μm.
[0030] The present application also discloses a method for manufacturing a modified polytetrafluoroethylene bearing material, comprising the following steps: Mix polytetrafluoroethylene, polyphenylene ester, modified wollastonite mineral fiber and hexagonal boron nitride together, blend them mechanically, and dry the mixed powder at 90° for 6 hours. Weigh the mixed and dried powder according to the weight percentage, spread it on the copper wire pad in the mold, and preform it by cold pressing on a hydraulic press. The pressure is 50-70MPa / cm 2 , keep the pressure for 3-5min. Take out the preformed blank from the mold, put it into the vacuum sintering furnace for heating and sintering, the sintering temperature is 360℃-395℃, keep the temperature for 40min-55min, and take it out of the furnace when it cools to less than 80℃.
[0031] Embodiment 1:
[0032] (1) PTFE 70%, POB 15%, MWF fiber 10%, H-BN particles 5% by weight, mixed and dried at 90° for 6 hours.
[0033] (2) Place the mixed and dried powder on the copper wire pad in the mold and preform it by cold pressing on a hydraulic press. The pressure is 60MPa / cm 2 , maintain pressure for 5 minutes.
[0034] (3) Place the cold pressed preformed blank in a vacuum sintering furnace and heat it at 375°C for 50 minutes. Remove it from the furnace when it cools to less than 80°C.
[0035] Embodiment 2:
[0036] (1) According to the weight percentage, PTFE 70%, POB 10%, MWF fiber 10%, H-BN particles 7% were mixed and dried at 90° for 6 hours.
[0037] (2) Place the mixed and dried powder on the copper wire pad in the mold and preform it by cold pressing on a hydraulic press. The pressure is 50MPa / cm 2 , maintain pressure for 3 minutes.
[0038] (3) Place the cold pressed preformed blank into a vacuum sintering furnace for heating and sintering at a temperature of 380°C for 45 minutes, and remove it from the furnace when it cools to less than 80°C.
[0039] Embodiment 3:
[0040] (1) According to the weight percentage, PTFE 65%, POB 18%, MWF fiber 13%, H-BN particles 4% were mixed and dried at 90° for 6 hours.
[0041] (2) Place the mixed and dried powder on the copper wire pad in the mold and preform it on a hydraulic press with a pressure of 55 MPa / cm 2, maintain pressure for 4 minutes.
[0042] (3) Place the cold pressed preformed blank into a vacuum sintering furnace for heating and sintering at a temperature of 385°C for 50 minutes, and remove it from the furnace when it is cooled to less than 80°C.
[0043] Embodiment 4:
[0044] (1) According to the weight percentage, PTFE 83%, POB 10%, MWF fiber 5%, H-BN particles 2% are mixed and dried at a drying temperature of 90° for 6 hours.
[0045] (2) Place the mixed and dried powder on the copper wire pad in the mold and preform it on a hydraulic press with a pressure of 50 MPa / cm 2 , maintain pressure for 3 minutes.
[0046] (3) Place the cold pressed preformed blank into a vacuum sintering furnace for heating and sintering at a temperature of 360°C for 55 minutes, and remove it from the furnace when it is cooled to less than 80°C.
[0047] Embodiment 5:
[0048] (1) According to the weight percentage, PTFE 57%, POB 20%, MWF fiber 15%, H-BN particles 8% are mixed and dried at a drying temperature of 90° for 6 hours.
[0049] (2) Place the mixed and dried powder on the copper wire pad in the mold and preform it on a hydraulic press with a pressure of 65MPa / cm 2 , maintain pressure for 4 minutes.
[0050] (3) Place the cold pressed preformed blank into a vacuum sintering furnace for heating and sintering at a temperature of 395°C for 40 minutes, and remove it from the furnace when it is cooled to less than 80°C.
[0051] The production process of modified polytetrafluoroethylene bearing materials is simple and the quality is easy to control. In particular, white fillers are selected to replace carbon fiber, graphite, and molybdenum disulfide, avoiding the use of black fillers and eliminating color pollution of the product. What is particularly important is that the selected inorganic fillers are inexpensive, the cost of product raw materials is low, and the price is competitive. The fillers are non-toxic, odorless, safe and environmentally friendly. The present invention effectively improves the mechanical properties and friction and wear properties of polytetrafluoroethylene bearing materials through the synergistic modification of organic and inorganic fillers. It is a highly wear-resistant, high-strength polymer bearing material and has a good prospect for promotion and application in fluid dynamic lubrication rotating equipment.
[0052] The tile surface made of the modified polytetrafluoroethylene bearing material of the present invention is brazed to a metal matrix steel tile base to obtain a metal-plastic composite sliding bearing composed of the modified polytetrafluoroethylene bearing material tile surface and the metal matrix steel tile base. The manufactured sliding bearing combines the rigidity of metal and the self-lubricating property of modified polytetrafluoroethylene. The mechanical properties and friction and wear properties are unified. The resin layer of the modified polytetrafluoroethylene bearing tile surface of the present invention is relatively thick, which can be 3-5mm, and various large-scale bearings with high load and high specific pressure can be manufactured, which can meet the various technical requirements of fluid dynamic pressure lubrication rotating equipment.
[0053] The modified polytetrafluoroethylene bearing materials prepared in Examples 1-5 of the present application are used as raw materials to prepare the metal-plastic composite sliding bearings of Examples 1-5 respectively. The composite sliding bearing prepared from the existing PTFE composite material with glass fiber added is used as Comparative Example 1, the composite sliding bearing prepared from the existing PTFE composite material with graphite added is used as Comparative Example 2, the composite sliding bearing prepared from the existing PTFE composite material with molybdenum disulfide added is used as Comparative Example 3, and the composite sliding bearing prepared from the existing PTFE composite material with carbon fiber added is used as Comparative Example 4. The sliding bearings of the 9 different embodiments obtained above are tested for performance and compared. As shown in the following table, the sliding bearings made of the modified polytetrafluoroethylene bearing material of the present application have a significant improvement in performance compared with the existing materials currently on the market.
[0054] Table 1 Comparison of test results of sliding bearings made of different materials Example 1 Example 2 Example 3 Example 4 Example 5 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Compressive strength MPa 52 51 50 50 51 44 45 46 46 Friction coefficient (dry friction) 0.12 0.13 0.13 0.16 0.15 0.18 0.15 0.17 0.14 Friction coefficient (oil dripping) 0.01 0.01 0.02 0.01 0.02 0.03 0.04 0.04 0.05 <![CDATA[Wear coefficient (oil dripping) cm 3 / N.m]]> <![CDATA[2*10 -11 ]]> <![CDATA[3*10 -11 ]]> <![CDATA[4*10 -11 ]]> <![CDATA[3*10 -11 ]]> <![CDATA[5*10 -11 ]]> <![CDATA[9*10 -11 ]]> <![CDATA[8*10 -11 ]]> <![CDATA[9*10 -11 ]]> <![CDATA[9*10 -11 ]]> <![CDATA[Coefficient of wear (dry friction) cm 3 / N.m]]> <![CDATA[3*10 -10 ]]> <![CDATA[4*10 -10 ]]> <![CDATA[5*10 -10 ]]> <![CDATA[4*10 -10 ]]> <![CDATA[6*10 -10 ]]> <![CDATA[2*10 -9 ]]> <![CDATA[1*10 -9 ]]> <![CDATA[2*10 -9 ]]> <![CDATA[1*10 -9 ]]> Allowable pressure MPa 10 9 8 7 8 8 6 7 Allowable PV value MPa.m / s 150 135 140 130 145 110 90 100 120 Tile surface limit operating temperature ℃ 130 120 115 110 120 109 106 108 110 The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the above embodiments do not limit the present invention in any form, and any technical solution obtained by equivalent replacement or equivalent transformation falls within the protection scope of the present invention.
Claims
1. A modified polytetrafluoroethylene bearing material, characterized in that: It is composed of polytetrafluoroethylene, polyphenylene ester, modified wollastonite mineral fiber and hexagonal boron nitride; The weight percentages of the various components are as follows: The polytetrafluoroethylene powder accounts for 57-83%, the polyphenyl ester powder accounts for 10-20%, the modified wollastonite mineral fiber accounts for 5-15%, and the hexagonal boron nitride particles account for 2-8%.
2. The modified polytetrafluoroethylene bearing material according to claim 1, characterized in that: The polytetrafluoroethylene powder accounts for 65-75%, the polyphenyl ester powder accounts for 13-17%, the modified wollastonite mineral fiber accounts for 8-12%, and the hexagonal boron nitride particles account for 3-7%.
3. The modified polytetrafluoroethylene bearing material according to claim 1, characterized in that: The particle size of the polytetrafluoroethylene powder is 20-70 μm, the particle size of the polyphenyl ester powder is 20-50 μm, the particle size of the modified wollastonite mineral fiber is 4-13 μm, the aspect ratio is 15:1, and the particle size of the hexagonal boron nitride is 1-5 μm.
4. The modified polytetrafluoroethylene bearing material according to claim 3, characterized in that: The particle size of the polytetrafluoroethylene powder is 40-60 μm, the particle size of the polyphenyl ester powder is 30-40 μm, the particle size of the modified wollastonite mineral fiber is 7-10 μm, the aspect ratio is 15:1, and the particle size of the hexagonal boron nitride is 1-5 μm.
5. A method for manufacturing a modified polytetrafluoroethylene bearing material according to any one of claims 1 to 4, characterized in that: The following steps are included: (1) Mix the above polymer materials and filler materials together in a certain proportion, mix them thoroughly and evenly by mechanical blending, and dry the mixed powder; (2) Place the prepared copper wire pad into the mold, spread the mixed and dried powder on the copper wire pad, and place it on a hydraulic press for cold pressing and preforming; (3) The preformed and pressed blank is placed in a vacuum sintering furnace for heating and sintering, and then taken out of the furnace after cooling.
6. The method for producing a modified polytetrafluoroethylene bearing material according to claim 5, characterized in that: The drying condition was 90°C for 6 hours.
7. The method for producing a modified polytetrafluoroethylene bearing material according to claim 5, characterized in that: The cold press preforming condition is a pressure of 50-70MPa / cm 2 , maintain pressure for 3-5 minutes.
8. The method for producing a modified polytetrafluoroethylene bearing material according to claim 5, characterized in that: The heating and sintering conditions are as follows: a sintering temperature of 360°C-395°C and a constant temperature of 40min-55min.
9. The method for producing a modified polytetrafluoroethylene bearing material according to claim 5, characterized in that: After heating and sintering, it is cooled to less than 80°C before being taken out of the furnace.
10. The method for producing a modified polytetrafluoroethylene bearing material according to claim 5, characterized in that: The prepared modified polytetrafluoroethylene bearing tile surface is brazed to the metal matrix steel tile base to obtain a metal plastic sliding bearing composed of the modified polytetrafluoroethylene bearing material tile surface and the metal matrix steel tile base.
Citation Information
Patent Citations
Polytetrafluoroethylene composite friction material and preparation method thereof
CN102942757A
Metal plastic composite bearing pad and manufacturing method thereof
CN102979819A
High-heat-resistance low-friction wollastonite fiber modified polytetrafluoroethylene lubricating material and preparation method thereof
CN117209930A
Spherical surface supporting elastic metallic plastic tile thrust bearing
CN201125937Y
Sliding bearing compound material and sliding bearing element made of same