Epoxy resin adhesive and preparation method thereof

By using synergistic enhancement technology of lignin, polyamic acid and composite filler in epoxy resin adhesive, the problem of insufficient bonding strength and temperature resistance of epoxy resin adhesive in electronic components is solved, and the further development is achieved High bonding strength and high temperature resistance.

CN119039912APending Publication Date: 2024-11-29SHENZHEN FRD SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411185326.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The bonding strength and temperature resistance of existing epoxy resin adhesives in electronic components are insufficient, especially when the structure is newly formed and miniaturized, resulting in poor bonding effect.

Method used

A combination formula of an epoxy resin adhesive is adopted, including 20-40 parts of epoxy resin, 10-15 parts of polyamic acid, 20-30 parts of composite filler, 10-15 parts of curing agent, 3-5 parts of lignin , 3-8 parts of diluent, 5-10 parts of toughening agent, and mixing through stirring, lignin, polyamic acid and composite filler are used to enhance the bonding strength and improve compatibility and dispersion.

Benefits of technology

It significantly improves the bonding strength and temperature resistance of epoxy resin adhesives, enhances mechanical properties, and ensures efficient bonding and high temperature resistance of electronic components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses an epoxy resin adhesive and a preparation method thereof. The epoxy resin adhesive comprises the following components in parts by mass: 20-40 parts of epoxy resin, 10-15 parts of polyamide acid, 20-30 parts of composite filler, 10-15 parts of a curing agent, 3-5 parts of lignin, 3-8 parts of a diluent and 5-10 parts of a flexibilizer. The lignin, the polyamide acid and the composite filler are utilized to synergistically enhance the bonding strength of the epoxy resin adhesive, and meanwhile, the polyamide acid and the epoxy resin are complementary, so that the temperature resistance of the epoxy resin adhesive is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of epoxy resins, and in particular to an epoxy resin adhesive and a preparation method thereof. Background Art

[0002] Epoxy resin is the most widely used matrix material in coatings, casting materials, adhesives, molding materials, injection molding materials and composite materials. It has the advantages of strong adhesion, high mechanical strength, excellent dielectric properties, good chemical corrosion resistance, etc. It has developed rapidly in recent years. Epoxy resin adhesive is an important variety of structural adhesives.

[0003] The epoxy glue currently used in electronic components does not meet the standards in terms of adhesion and impact resistance. In particular, as the structure of electronic components becomes more modern and miniaturized, the bonding area is reduced. At the same time, due to the poor temperature resistance of epoxy resin, the bonding effect of electronic component adhesives is poor.

[0004] Therefore, it is necessary to provide an epoxy adhesive with high bonding strength and good temperature resistance. Summary of the invention

[0005] In view of the defects in the prior art, the present invention provides an epoxy resin adhesive and a preparation method thereof, so as to solve the problem of how to improve the bonding strength and temperature resistance of the epoxy adhesive.

[0006] In order to solve the above technical problems, this application proposes the following technical solutions:

[0007] In a first aspect, the present application provides an epoxy resin adhesive comprising the following components in parts by weight: 20-40 parts of epoxy resin, 10-15 parts of polyamic acid, 20-30 parts of composite filler, 10-15 parts of curing agent, 3-5 parts of lignin, 3-8 parts of diluent, and 5-10 parts of toughening agent.

[0008] Preferably, the composite filler includes 50 parts of calcium carbonate, 20-30 parts of mica powder, and 20-30 parts of bentonite.

[0009] Preferably, the curing agent includes one or more of 2-methylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, and 1-cyanoethyl-2-phenylimidazole.

[0010] Preferably, the diluent includes one or more of benzyl glycidyl ether, neodecanoic acid glycidyl ester, and phenyl glycidyl ether.

[0011] Preferably, the toughening agent comprises eleostearic anhydride.

[0012] Preferably, the mass ratio of toughener to epoxy resin and diluent is 10:20-40:3.

[0013] Preferably, the average particle size of calcium carbonate is 0.5-3 μm, the average particle size of mica powder is 8-15 μm, and the average particle size of bentonite is 22-30 μm.

[0014] In a second aspect, the present application provides a method for preparing an epoxy resin adhesive, comprising the following steps: stirring and mixing polyamic acid, lignin, a diluent, a toughening agent, and a composite filler once, and then adding a curing agent and an epoxy resin and stirring and mixing them a second time to obtain the epoxy resin adhesive.

[0015] Preferably, the temperature of the first stirring is 50-70°C, and the temperature of the second stirring is 25-35°C.

[0016] In a third aspect, the present application provides an application of an epoxy resin adhesive in the preparation of electronic components.

[0017] In summary, compared with the prior art, the present invention achieves the following technical effects: the present application utilizes lignin, polyamic acid and composite fillers to synergistically enhance the bonding strength of epoxy resin adhesives. The reason is that lignin can be used as an organic modifier for calcium carbonate and polyamic acid, and interacts with calcium carbonate and polyamic acid in the composite filler through its rich active groups, thereby improving the compatibility and dispersibility of the composite filler, polyamic acid and epoxy resin matrix, and enhancing the viscosity of the epoxy resin. In addition, lignin improves the mechanical properties of the composite filler, thereby improving the bonding strength of the epoxy resin adhesive. DETAILED DESCRIPTION

[0018] In order to enable those skilled in the art to better understand the solutions of the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only embodiments of a part of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0019] In a first aspect, the present application provides an epoxy resin adhesive comprising the following components in parts by weight: 20-40 parts of epoxy resin, 10-15 parts of polyamic acid, 20-30 parts of composite filler, 10-15 parts of curing agent, 3-5 parts of lignin, 3-8 parts of diluent, and 5-10 parts of toughening agent.

[0020] In the present application, the epoxy resin has good adhesion performance but poor high temperature resistance, while the polyamic acid has good high temperature resistance but low bonding strength. The overall adhesion and high temperature resistance of the adhesive can be improved by the complementarity of the epoxy resin and the polyamic acid. However, the improvement of the temperature resistance will lead to a decrease in viscosity, thereby affecting the overall bonding ability. In order to overcome the above-mentioned defects, the present application utilizes lignin, polyamic acid and composite fillers to synergistically enhance the bonding strength of the epoxy resin adhesive. The reason is that lignin can be used as an organic modifier of calcium carbonate and polyamic acid, and interacts with calcium carbonate and polyamic acid in the composite filler through its rich active groups, thereby improving the compatibility and dispersibility of the composite filler, polyamic acid and the epoxy resin matrix, and enhancing the viscosity of the epoxy resin. In addition, lignin improves the mechanical properties of the composite filler, thereby improving the bonding strength of the epoxy resin adhesive.

[0021] In some embodiments, the composite filler includes 50 parts of calcium carbonate, 20-30 parts of mica powder, and 20-30 parts of bentonite.

[0022] In this embodiment, by adding mica powder and bentonite, the viscosity of the adhesive is increased, the shrinkage rate is reduced, the adsorption and convergence effect is enhanced, and the size and structure of the adhesive film during the curing process of the epoxy adhesive are controlled, which is beneficial to enhancing the bonding strength of the epoxy resin adhesive.

[0023] In some embodiments, the curing agent includes one or more of 2-methylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, and 1-cyanoethyl-2-phenylimidazole.

[0024] In some embodiments, the diluent includes one or more of benzyl glycidyl ether, neodecanoic acid glycidyl ester, and phenyl glycidyl ether.

[0025] In some embodiments, the toughening agent includes eleostearic anhydride.

[0026] In this embodiment, tung oil anhydride is used to partially toughen the epoxy resin, which is beneficial to improving the bonding strength of the epoxy resin adhesive.

[0027] In some embodiments, the mass ratio of toughening agent to epoxy resin and diluent is 10:20-40:3.

[0028] In this embodiment, the amount of toughening agent is controlled to ensure that the toughening agent reacts with part of the groups of the epoxy resin and the diluent, while the remaining epoxy groups can still react with the curing agent.

[0029] In some embodiments, the average particle size of calcium carbonate is 0.5-3 μm, the average particle size of mica powder is 8-15 μm, and the average particle size of bentonite is 22-30 μm.

[0030] In a second aspect, the present application provides a method for preparing an epoxy resin adhesive, comprising the following steps: stirring and mixing polyamic acid, lignin, a diluent, a toughening agent, and a composite filler once, and then adding a curing agent and an epoxy resin and stirring and mixing them a second time to obtain the epoxy resin adhesive.

[0031] In some embodiments, the temperature of the first stirring is 50-70°C, and the temperature of the second stirring is 25-35°C.

[0032] In this embodiment, the temperature of the first stirring is higher than the temperature of the second stirring. During the first stirring, the polyamic acid, lignin, diluent, toughening agent, and composite filler have strong temperature resistance. After being fully reacted and mixed, they react with the epoxy resin and curing agent to avoid denaturation of the epoxy resin.

[0033] In a third aspect, the present application provides an application of an epoxy resin adhesive in the preparation of electronic components.

[0034] The present solution is further described below through specific implementation methods.

[0035] Example 1

[0036] An epoxy resin adhesive comprises the following components by mass: 20g of epoxy resin (CAS: 61788-97-4), 10g of polyamic acid, 20g of composite filler, 10g of 2-methylimidazole, 3g of lignin, 3g of benzyl glycidyl ether, and 10g of tung oil anhydride; the composite filler comprises 10g of calcium carbonate with a particle size of 2μm, 4g of mica powder with a particle size of 10μm, and 6g of bentonite with a particle size of 25μm.

[0037] A preparation method of an epoxy resin adhesive comprises the following steps: stirring polyamic acid, lignin, benzyl glycidyl ether, tung oil anhydride and a composite filler at 70°C for 5 hours, adding 2-methylimidazole and epoxy resin and stirring for 2 hours at 25°C to obtain the epoxy resin adhesive.

[0038] Example 2

[0039] An epoxy resin adhesive comprises the following components in parts by mass: 40g of epoxy resin, 15 parts of polyamic acid, 20g of composite filler, 15g of 1-cyanoethyl-2-phenylimidazole, 5 parts of lignin, 3g of glycidyl neodecanoate, and 5g of tung oil anhydride; the composite filler comprises 10g of calcium carbonate with a particle size of 2μm, 4g of mica powder with a particle size of 10μm, and 6g of bentonite with a particle size of 25μm.

[0040] A preparation method of an epoxy resin adhesive comprises the following steps: stirring polyamic acid, lignin, neodecanoic acid glycidyl ester, tung oil anhydride and a composite filler at 70°C for 5 hours, adding 1-cyanoethyl-2-phenylimidazole and epoxy resin and continuing to stir for a second time at 25°C for 2 hours to obtain the epoxy resin adhesive.

[0041] Example 3

[0042] An epoxy resin adhesive comprises the following components by mass: 20g of epoxy resin (CAS: 61788-97-4), 10g of polyamic acid, 20g of composite filler, 10g of 2-methylimidazole, 3g of lignin, 3g of benzyl glycidyl ether, and 5g of tung oil anhydride; the composite filler comprises 10g of calcium carbonate with a particle size of 0.5μm, 4g of mica powder with a particle size of 8μm, and 6g of bentonite with a particle size of 30μm.

[0043] A preparation method of an epoxy resin adhesive comprises the following steps: stirring polyamic acid, lignin, benzyl glycidyl ether, tung oil anhydride and a composite filler at 60°C for 5 hours and mixing them evenly, then adding 2-methylimidazole and epoxy resin and stirring them again at 30°C for 2 hours and mixing them evenly to obtain the epoxy resin adhesive.

[0044] Comparative Example 1

[0045] An epoxy resin adhesive comprises the following components by mass: 20g of epoxy resin (CAS: 61788-97-4), 20g of composite filler, 10g of 2-methylimidazole, 3g of lignin, 3g of benzyl glycidyl ether, and 10g of tung oil anhydride; the composite filler comprises 10g of calcium carbonate with a particle size of 2μm, 4g of mica powder with a particle size of 10μm, and 6g of bentonite with a particle size of 25μm.

[0046] A preparation method of an epoxy resin adhesive comprises the following steps: stirring lignin, benzyl glycidyl ether, tung oil anhydride and a composite filler at 70°C for 5 hours, adding 2-methylimidazole and epoxy resin and stirring for 2 hours at 25°C to obtain the epoxy resin adhesive.

[0047] Comparative Example 2

[0048] An epoxy resin adhesive comprises the following components in parts by mass: 20g of epoxy resin (CAS: 61788-97-4), 10g of polyamic acid, 20g of calcium carbonate, 10g of 2-methylimidazole, 3g of lignin, 3g of benzyl glycidyl ether, and 10g of tung oil anhydride.

[0049] A preparation method of an epoxy resin adhesive comprises the following steps: stirring polyamic acid, lignin, benzyl glycidyl ether, tung oil anhydride and calcium carbonate at 70°C for 5 hours, adding 2-methylimidazole and epoxy resin and stirring for 2 hours at 25°C to obtain the epoxy resin adhesive.

[0050] Comparative Example 3

[0051] An epoxy resin adhesive comprises the following components by mass: 20g of epoxy resin (CAS: 61788-97-4), 10g of polyamic acid, 20g of composite filler, 10g of 2-methylimidazole, 3g of benzyl glycidyl ether, and 10g of tung oil anhydride; the composite filler comprises 10g of calcium carbonate with a particle size of 2μm, 4g of mica powder with a particle size of 10μm, and 6g of bentonite with a particle size of 25μm.

[0052] A preparation method of an epoxy resin adhesive comprises the following steps: stirring polyamic acid, benzyl glycidyl ether, tung oil anhydride and a composite filler at 70°C for 5 hours, adding 2-methylimidazole and epoxy resin and stirring for 2 hours at 25°C to obtain the epoxy resin adhesive.

[0053] Comparative Example 4

[0054] An epoxy resin adhesive comprises the following components by mass: 20g of epoxy resin (CAS: 61788-97-4), 10g of polyamic acid, 20g of composite filler, 10g of 2-methylimidazole, 3g of lignin, and 3g of benzyl glycidyl ether; the composite filler comprises 10g of calcium carbonate with a particle size of 2μm, 4g of mica powder with a particle size of 10μm, and 6g of bentonite with a particle size of 25μm.

[0055] A preparation method of an epoxy resin adhesive comprises the following steps: stirring polyamic acid, lignin, benzyl glycidyl ether and a composite filler at 70°C for 5 hours, adding 2-methylimidazole and epoxy resin and stirring for 2 hours at 25°C to obtain the epoxy resin adhesive.

[0056] Comparative Example 5

[0057] An epoxy resin adhesive comprises the following components by mass: 20g of epoxy resin (CAS: 61788-97-4), 10g of polyamic acid, 20g of composite filler, 10g of 2-methylimidazole, 3g of lignin, 3g of benzyl glycidyl ether, and 20g of tung oil anhydride; the composite filler comprises 10g of calcium carbonate with a particle size of 2μm, 4g of mica powder with a particle size of 10μm, and 6g of bentonite with a particle size of 25μm.

[0058] A preparation method of an epoxy resin adhesive comprises the following steps: stirring polyamic acid, lignin, benzyl glycidyl ether, tung oil anhydride and a composite filler at 70°C for 5 hours, adding 2-methylimidazole and epoxy resin and stirring for 2 hours at 25°C to obtain the epoxy resin adhesive.

[0059] Test and Evaluation

[0060] The bonding performance and temperature resistance of the epoxy resin adhesives obtained in the embodiments and comparative examples were tested, and the results are shown in Table 1.

[0061] Table 1 Test results

[0062]

[0063]

[0064] The above test data show that the present application utilizes lignin, polyamic acid and composite filler to synergistically enhance the bonding strength of epoxy resin adhesive. The reason is that lignin can be used as an organic modifier for calcium carbonate and polyamic acid, and interacts with calcium carbonate and polyamic acid in the composite filler through its rich active groups, thereby improving the compatibility and dispersibility of the composite filler, polyamic acid and epoxy resin matrix, and enhancing the viscosity of the epoxy resin. In addition, lignin improves the mechanical properties of the composite filler, thereby improving the bonding strength of the epoxy resin adhesive.

[0065] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. An epoxy resin adhesive, characterized in that: The invention comprises the following components in parts by weight: 20-40 parts of epoxy resin, 10-15 parts of polyamic acid, 20-30 parts of composite filler, 10-15 parts of curing agent, 3-5 parts of lignin, 3-8 parts of diluent and 5-10 parts of toughening agent.

2. The epoxy resin adhesive according to claim 1, characterized in that: The composite filler comprises 50 parts of calcium carbonate, 20-30 parts of mica powder and 20-30 parts of bentonite.

3. The epoxy resin adhesive according to claim 1, characterized in that: The curing agent includes one or more of 2-methylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, and 1-cyanoethyl-2-phenylimidazole.

4. The epoxy resin adhesive according to claim 1, characterized in that: The diluent includes one or more of benzyl glycidyl ether, neodecanoic acid glycidyl ester and phenyl glycidyl ether.

5. The epoxy resin adhesive according to claim 1, characterized in that: The toughening agent includes tung oil anhydride.

6. The epoxy resin adhesive according to claim 1, characterized in that: The mass ratio of the toughening agent to the epoxy resin and the diluent is 10:20-40:

3.

7. The epoxy resin adhesive according to claim 2, characterized in that: The average particle size of the calcium carbonate is 0.5-3 μm, the average particle size of the mica powder is 8-15 μm, and the average particle size of the bentonite is 22-30 μm.

8. A method for preparing the epoxy resin adhesive according to any one of claims 1 to 7, characterized in that: The method comprises the following steps: stirring and mixing polyamic acid, lignin, diluent, toughening agent and composite filler once, adding curing agent and epoxy resin and stirring and mixing again to obtain the epoxy resin adhesive.

9. The preparation method according to claim 8, characterized in that: The temperature of the first stirring is 50-70°C, and the temperature of the second stirring is 25-35°C.

10. Use of the epoxy resin adhesive according to any one of claims 1 to 7 in the preparation of electronic components.