Organic long afterglow material, preparation method and application of organic long afterglow material in three-level encryption

By doping host materials and guest materials with different melting points and crystallinity, organic long afterglow materials with multiple lifespan, color and temperature stimulation responses were prepared, and a three-level encryption system was constructed, which solved the poor encryption effect in the existing technology. Problem, high-level information encryption and anti-counterfeiting applications are realized.

CN119039974APending Publication Date: 2024-11-29HEFEI HUISHI TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411175789.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The prior art is difficult to construct organic long afterglow materials with multiple lifespan, color and temperature stimulation responses, limiting their application potential in the fields of information encryption and anti-counterfeiting.

Method used

By selecting host materials with different melting points and good crystallinity doping with guest materials with different afterglow color potential, an organic long afterglow material with multiple lifetimes, color and temperature stimulation responses were prepared by the water matrix method and based on these Features to build a three-level encryption system.

Benefits of technology

It achieves a high-level encryption effect, is not easy to forge, and can be used through cooling and recycling after heating and deactivation, expanding the application scenarios of organic afterglow materials in the fields of information encryption and anti-counterfeiting.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039974A_ABST
    Figure CN119039974A_ABST
Patent Text Reader

Abstract

The invention discloses an organic long-afterglow material with multi-life, color and temperature stimulation response, and a preparation method and application thereof, and the organic long-afterglow material is formed by doping host materials with different melting points and good crystallinity and guest materials with different afterglow color potentials. The host materials are triphenylphosphine (TPP) and diphenylamine (DPA), and the guest materials are selected from biphenyl derivatives. According to the invention, on the basis of multiple life, color and temperature stimulation response characteristics of the organic long afterglow material, a time, color and temperature three-level encryption system is constructed; the encryption system disclosed by the invention is high in encryption grade and not easy to counterfeit, so that the organic long-afterglow material can be widely applied in the aspects of information encryption and anti-counterfeiting.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of room temperature phosphorescence (RTP) materials, in particular to an organic long afterglow material, a preparation method and application in three-level encryption. Background Art

[0002] At present, a large number of inorganic long afterglow material systems have been developed, and the preparation process of inorganic long afterglow materials has also matured. Compared with inorganic long afterglow materials, organic long afterglow materials have many advantages such as diverse structures, simple manufacturing processes, low manufacturing costs, and good compatibility with various matrices. The advantages in various fields have made organic long afterglow materials gradually become the focus and hotspot of current research. Whether in system design and preparation, mechanism research with general guiding significance, or practical application, organic long afterglow materials have very important research value.

[0003] Organic long afterglow materials are widely used due to their unique advantages, such as information encryption and anti-counterfeiting, programmable labels, 3D and thermal printing, sensors and bio-imaging, and afterglow organic light-emitting diodes (OLEDs), etc. Among them, information security has always been a focus of attention, and the advancement of science and technology has also prompted researchers to continuously seek new information encryption and anti-counterfeiting technologies. Organic long afterglow materials have become ideal materials for the development of encryption and anti-counterfeiting technology due to their unique optical lifetime, color, and external stimulus response characteristics. Therefore, the use of multiple lifetimes, colors, and external stimulus response characteristics of organic long afterglow materials to construct multi-level encryption will greatly improve the practical application of organic long afterglow materials in the fields of information encryption and anti-counterfeiting.

[0004] Therefore, an organic long afterglow material with multiple lifetimes, colors and stimulus responses was constructed, and based on the multiple lifetimes, colors and temperature stimulus response characteristics of the organic long afterglow material, a three-level encryption system was constructed and applied. Summary of the invention

[0005] In view of the deficiencies in the prior art, the purpose of the present invention is to construct an organic long afterglow material with multiple lifetimes, colors and temperature stimulus responses and a preparation method thereof, and based on the multiple lifetimes, colors and temperature stimulus response characteristics of the organic long afterglow material, a three-level encryption system is constructed and applied.

[0006] Another object of the present invention is to provide an organic long afterglow material with multiple lifetimes, colors and temperature stimulus responses and a preparation method thereof.

[0007] Another object of the present invention is to provide a series of organic long afterglow materials having multiple lifetimes, colors and temperature stimulus responses and a preparation method thereof.

[0008] Another object of the present invention is to provide an application of organic long afterglow materials in three-level encryption.

[0009] The purpose of the present invention is achieved through the following technical solutions.

[0010] In the above technical solution, the decryption procedure may include differences in time, temperature and color.

[0011] An organic long afterglow material with multiple lifespans, colors and temperature stimulus responses, characterized in that it is made by doping a host material with different melting points and good crystallinity with a guest material with different afterglow color potentials.

[0012] The organic long afterglow material with multiple lifetimes, colors and temperature stimulus responses is characterized in that the main materials are triphenylphosphine (TPP) and diphenylamine (DPA) respectively.

[0013] The organic long afterglow material with multiple lifetimes, colors and temperature stimulus responses is characterized in that the guest material is a biphenyl derivative.

[0014] The organic long afterglow material with multiple lifetimes, colors and temperature stimulus responses is characterized in that the biphenyl derivative refers to N,N'-diphenyl-N,N'-(1-naphthyl)-1,1'-biphenyl-4,4'-diamine (NPD), N,N,N'-triphenylbenzidine (NTPB), N,N'-diphenylbenzidine (NDPB),

[0015]

[0016] The organic long afterglow material with multiple lifetimes, colors and temperature stimulus responses is characterized in that the host materials are triphenylphosphine and diphenylamine, respectively, and the guest materials refer to N,N'-diphenyl-N,N'-(1-naphthyl)-1,1'-biphenyl-4,4'-diamine, N,N,N'-triphenylbenzidine, and N,N'-diphenylbenzidine; the following six materials are doped: triphenylphosphine: N,N'-diphenyl-N,N'-(1-naphthyl)-1,1'-biphenyl-4,4'-diamine, triphenylphosphine and N,N,N'-triphenylbenzidine, triphenylphosphine and N,N'-diphenylbenzidine, diphenylamine and N,N'-diphenyl-N,N'-(1-naphthyl)-1,1'-biphenyl-4,4'-diamine, diphenylamine and N,N,N'-triphenylbenzidine, and diphenylamine: N,N'-diphenylbenzidine.

[0017] The organic long afterglow material with multiple lifespans, colors and temperature stimulus responses is characterized in that the molar ratio of the host material to the guest material is 80-100:1.

[0018] The method for preparing the organic long afterglow material with multiple lifespans, colors and temperature stimulus responses is characterized in that the organic long afterglow material is prepared by a water matrix method.

[0019] The method for preparing an organic long afterglow material with multiple lifespans, colors and temperature stimulus responses is characterized in that triphenylphosphine: N,N'-diphenyl-N,N'-(1-naphthyl)-1,1'-biphenyl-4,4'-diamine, triphenylphosphine and N,N,N'-triphenylbenzidine, triphenylphosphine and N,N'-diphenylbenzidine are used to prepare the organic long afterglow material using a water matrix method, and the heating temperature in water is 80°C; diphenylamine and N,N'-diphenyl-N,N'-(1-naphthyl)-1,1'-biphenyl-4,4'-diamine, diphenylamine and N,N,N'-triphenylbenzidine, diphenylamine: N,N'-diphenylbenzidine is used to prepare the organic long afterglow material using a water matrix method, and the heating temperature in water is 55°C.

[0020] The application of organic long afterglow materials with multiple lifetimes, colors and temperature stimulus responses in three-level encryption is characterized in that it includes the preparation of an adhesive, the adhesive is used for initial input of information, and the luminescent material prepared according to one of claims 5-8 is used for attachment encryption as needed.

[0021] The application of the organic long afterglow material with multiple lifespans, colors and temperature stimulus responses in three-level encryption is characterized in that the adhesive is prepared by: making an aqueous solution of polyvinyl pyrrolidone.

[0022] Reasonable design of decryption procedures will greatly expand the practicality of this strategy in the field of information encryption. This encryption strategy shows great application potential.

[0023] The beneficial effects of the present invention are as follows:

[0024] 1. By selecting host materials with different melting points and good crystallinity, selecting guest materials with different afterglow color potential, and further doping with a variety of host materials with different melting points, a series of long afterglow materials with temperature stimulus response, multicolor and time resolution are constructed;

[0025] 2. Based on the multiple lifespans, colors and temperature stimulus response characteristics of organic long afterglow materials, the present invention constructs a three-level encryption system of time, color and temperature;

[0026] 3. The encryption system of the present invention has a high encryption level and is not easy to forge, so that organic long afterglow materials are more widely used in information encryption and anti-counterfeiting;

[0027] 4. The encryption system of the present invention can be cooled and recycled after being inactivated by heating, which greatly improves its practical application scenarios. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is a performance display diagram of the long afterglow luminescent material with multiple lifetimes, colors and temperature responses prepared in Example 3 of the present invention;

[0029] Figure 2 is a semi-logarithmic graph of the emission decay curve of the long afterglow material prepared in Example 3 of the present invention;

[0030] Figure 3 It is the steady-state emission spectrum of the long afterglow material and the corresponding host and guest materials in the present invention;

[0031] Figure 4 This is an information display diagram obtained by using the decryption method in Example 6 in Example 5 of the present invention;

[0032] Figure 5 It is a display of the encryption application prepared in Example 6 of the present invention. DETAILED DESCRIPTION

[0033] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0034] A strategy for constructing organic long afterglow materials with multiple lifetimes, colors and temperature stimulus responses: select host materials with different melting points and good crystallinity, select guest materials with different afterglow color potentials to dope with the host materials, and construct a series of long afterglow materials with temperature stimulus response, multicolor and time resolution.

[0035] In order to construct a multi-level temperature stimulus response system, host materials with different melting points were selected, namely triphenylphosphine (TPP) and diphenylamine (DPA). In view of the excellent RTP luminescence potential of biphenyl derivatives, a series of biphenyl derivatives N,N'-diphenyl-N,N'-(1-naphthyl)-1,1'-biphenyl-4,4'-diamine (NPD), N,N,N'-triphenylbenzidine (NTPB) and N,N'-diphenylbenzidine (NDPB) were selected as guest materials, as shown in the figure below.

[0036]

[0037] Six organic long afterglow materials, TPP:NPD, TPP:NTPB, TPP:NDPB, DPA:NPD, DPA:NTPB and DPA:NDPB, were prepared by water matrix method. Based on the multiple lifetime, color and temperature stimulus response characteristics of these six organic long afterglow materials, a three-level encryption system was constructed and applied.

[0038] In the above technical scheme, the molar ratio of the main material and the guest material is 100:1; the heating temperature of TPP:NPD, TPP:NTPB and TPP:NDPB in water is 80°C; the heating temperature of DPA:NPD, DPA:NTPB and DPA:NDPB in water is 55°C.

[0039] Application of organic long afterglow materials in three-level encryption:

[0040] The method includes the preparation of an adhesive, using the adhesive to input information for the first time, and attaching different luminescent materials according to needs.

[0041] In the above technical solution, the adhesive is prepared by adding 1.6 g of polyvinyl pyrrolidone (PVP) to 10 mL of aqueous solution and stirring at 50° C. for 3 h.

[0042] In the following examples, N,N'-diphenyl-N,N'-(1-naphthyl)-1,1'-biphenyl-4,4'-diamine (NPD), N,N'-diphenylbenzidine (NDPB) and diphenylamine (DPA) were purchased from San Chemical Technology Co., Ltd. (purity: 98%-99%); N,N,N'-triphenylbenzidine (NTPB) was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.; triphenylphosphine (TPP) was purchased from Anhui Zesheng Technology Co., Ltd. Polyvinylpyrrolidone (PVP) was purchased from Shandong Youso Chemical Technology Co., Ltd.

[0043] The instruments and models involved in the tests in the following embodiments are:

[0044] Ocean Optics multi-band spectrometer, FlexSEM 1000 scanning electron microscope, F-7000 fluorescence spectrometer;

[0045] Room temperature: 20~25℃.

[0046] The power of the UV lamp in the following examples is 20W (365nm).

[0047] Example 1

[0048] Screening of host materials: The host can provide a good rigid environment, inhibit the non-radiative attenuation of guest molecules, and thus enhance the luminescence performance of the host-guest LPL material. Therefore, it is very important to screen out host materials that can provide a good rigid environment. On this basis, host materials with different melting points are further screened out, and the difference in their melting points can be used to construct a series of LPL materials with different temperature stimulus responses. Therefore, we selected TPP (melting point 80°C) and DPA (melting point 53°C) with different melting points as host materials. Furthermore, both of them have good crystallinity.

[0049] Example 2

[0050] Screening of guest materials: Guest materials are the key to making host-guest LPL materials luminescent. Through a large amount of photophysical data verification, it can be concluded that the luminescence of host-guest LPL materials mainly comes from the internal guest molecules. Therefore, in order to construct LPL materials with different afterglow times and different afterglow colors, it is necessary to screen out guest molecules with different luminescent color potentials, and further utilize the differences in host molecules to achieve differences in afterglow time. Based on this, we selected NDPB and NTPB with green luminescence potential and NPD with yellow luminescence potential as guest materials to achieve multi-color afterglow.

[0051] Example 3

[0052] Triphenylphosphine (TPP) and N,N'-diphenyl-N,N'-(1-naphthyl)-1,1'-biphenyl-4,4'-diamine (NPD) powder (1 mol%) were added to 15 mL of water, and then heated and stirred at 80°C. After 15 minutes, the temperature was slowly lowered until crystals precipitated. The solution containing the crystals was filtered and dried to obtain TPP:NPD crystal powder. Similarly, the heating temperatures of the other five doped crystals were 80°C and 53°C for the main molecule triphenylphosphine and diphenylamine, respectively, and the other preparation conditions were the same.

[0053] Figure 1 This is a graph showing the luminescence performance of six organic long afterglow materials: TPP:NPD, TPP:NTPB, TPP:NDPB, DPA:NPD, DPA:NTPB and DPA:NDPB. It can be seen that the prepared doped crystals have afterglows of about 3s, 3.5s, 1s, 2.5s, 3.5s, and 4.5s, respectively.

[0054] Figure 2 From the semi-logarithmic graph of the emission decay curves of six organic long afterglow materials, TPP:NPD, TPP:NTPB, TPP:NDPB, DPA:NPD, DPA:NTPB and DPA:NDPB, it can be seen that the afterglow times of doped crystals TPP:p-TPD, TPA:p-TPD, DPA:p-TPD and PB:p-TPD are 4.5s, 2.0s, 3.0s and 2.2s, respectively, which is basically consistent with actual observations.

[0055] Figure 3These are the phosphorescence emission spectra of six organic long afterglow materials, TPP:NPD, TPP:NTPB, TPP:NDPB, DPA:NPD, DPA:NTPB and DPA:NDPB. As can be seen from the figure, the steady-state emission spectra of doped crystals TPP:NPD, TPP:NTPB, TPP:NDPB, DPA:NPD, DPA:NTPB and DPA:NDPB in the range of 470-700nm are basically consistent with the phosphorescence emission spectra of the guest molecules. Their corresponding maximum phosphorescence emission wavelengths are 532nm, 513nm, 517nm, 540nm, 515nm and 509nm, respectively, which are also basically close to the maximum phosphorescence emission wavelengths of 552nm, 514nm and 509nm of the guest molecules NPD, NTPB and NDPB. Therefore, the afterglow of the host-guest long afterglow luminescent material mainly comes from the guest molecules. Therefore, the strategy of constructing multicolor afterglow materials using different guest molecules is feasible.

[0056] Example 4

[0057] Preparation of adhesive: Add 1.6 g of polyvinyl pyrrolidone (PVP) to 10 mL of aqueous solution and stir at 50 °C for 3 h.

[0058] Example 5

[0059] We selected four groups of doped crystals, TPP:NPD, TPP:NTPB, DPA:NPD and DPA:NDPB, with good afterglow time difference, different melting points and afterglow colors, to construct a three-level encryption system. The number "2024" was written on the paper substrate using the adhesive prepared in Example 4, and the TPP:NPD long afterglow material was attached to the first number "2", the DPA:NPD long afterglow material was attached to the second number "0", the DPA:NDPB long afterglow material was attached to the third number "2", and the TPP:NTPB long afterglow material was attached to the fourth number "4".

[0060] Figure 4It is the encryption material prepared in Example 5. According to the decryption process and restoration process of Example 6, different encrypted information can be read. At room temperature, the number shows the word "2024" under the excitation of the light source. After turning off the excitation light source, as time goes by, the number gradually changes from "2024" to "224", then to "22", and finally to "2". We assume that the number is read once every 0.5s, and finally all the numbers are arranged in sequence to get the encrypted information. Then the information we want to convey in the end is "2024-224-224-24-24-2", that is, "202420242024224242". If it is assumed that the reading interval is 1s, the conveyed information is changed to "2024-224-224-2", that is, "202420242242". Subsequently, we heated it at 55°C for 5min, and found that the displayed information changed after exciting it again. Similarly, if the reading interval is 0.5s, the encrypted information changes to "24-24-24-24-2-2", that is, "2424242422". If the reading interval is 1s, the encrypted information changes to "24-24-2", that is, "24242". This is because the DPA in the doped crystals DPA:NPD and DPA:NDPB melts at 55°C and can no longer interact with the guest molecules, so the doped crystals lose their LPL performance. However, over time, the LPL performance of the doped crystals gradually recovers, showing a good reversible temperature response.

[0061] Example 6

[0062] Take the three-level encryption material prepared in Example 5, record the afterglow information at room temperature, heat it to 55° C., and record the afterglow information again. Finally, cool the three-level encryption material for 5 minutes to restore it to its initial state, and record the afterglow information again.

[0063] Example 7

[0064] Take six organic long afterglow materials, TPP:NPD, TPP:NTPB, TPP:NDPB, DPA:NPD, DPA:NTPB and DPA:NDPB, stir with PVP and aqueous solution until uniform dispersion, and finally obtain a white paste slurry. Among them, the mass fraction ratio of doped crystals to PVP is 2:3, and the mass fraction of PVP (mg) to the volume fraction of pure water (mL) is 10:1. The slurry is coated on the encryption matrix to realize information encryption application.

[0065] Figure 5 The slurry prepared in Example 7 is taken and written or screen-printed on a paper substrate, and then excited by an ultraviolet lamp and turned off to realize encryption application.

Claims

1. An organic long afterglow material with multiple lifetimes, colors and temperature stimulus responses, characterized in that: It is made by doping a host material with different melting points and good crystallinity with a guest material with different afterglow color potential.

2. The organic long afterglow material with multiple lifetimes, colors and temperature stimulus responses according to claim 1, characterized in that: The main materials are triphenylphosphine (TPP) and diphenylamine (DPA).

3. The organic long afterglow material with multiple lifetimes, colors and temperature stimulus responses according to claim 1, characterized in that: The guest material is selected from biphenyl derivatives.

4. The organic long afterglow material with multiple lifetimes, colors and temperature stimulus responses according to claim 1, characterized in that: The biphenyl derivatives are N,N'-diphenyl-N,N'-(1-naphthyl)-1,1'-biphenyl-4,4'-diamine (NPD), N,N,N'-triphenylbenzidine (NTPB), N,N'-diphenylbenzidine (NDPB), 。 5. The organic long afterglow material with multiple lifetimes, colors and temperature stimulus responses according to claim 1, characterized in that: The host materials are triphenylphosphine and diphenylamine, respectively, and the guest materials are N,N'-diphenyl-N,N'-(1-naphthyl)-1,1'-biphenyl-4,4'-diamine, N,N,N'-triphenylbenzidine, and N,N'-diphenylbenzidine; The following six materials were doped: triphenylphosphine: N,N'-diphenyl-N,N'-(1-naphthyl)-1,1'-biphenyl-4,4'-diamine, triphenylphosphine and N,N,N'-triphenylbenzidine, triphenylphosphine and N,N'-diphenylbenzidine, diphenylamine and N,N'-diphenyl-N,N'-(1-naphthyl)-1,1'-biphenyl-4,4'-diamine, diphenylamine and N,N,N'-triphenylbenzidine, diphenylamine: N,N'-diphenylbenzidine.

6. The organic long afterglow material with multiple lifetimes, colors and temperature stimulus responses according to claim 1 or 5, characterized in that: The molar ratio of the host material to the guest material is 80-100:

1.

7. The method for preparing an organic long afterglow material with multiple lifetimes, colors and temperature stimulus responses according to any one of claims 1 to 5, characterized in that: Organic long afterglow materials were prepared by water matrix method.

8. The method for preparing an organic long afterglow material with multiple lifetimes, colors and temperature stimulus responses according to claim 7, characterized in that: Triphenylphosphine: N,N'-diphenyl-N,N'-(1-naphthyl)-1,1'-biphenyl-4,4'-diamine, triphenylphosphine and N,N,N'-triphenylbenzidine, triphenylphosphine and N,N'-diphenylbenzidine are used to prepare organic long afterglow materials using a water matrix method, and the heating temperature in water is 80°C; diphenylamine and N,N'-diphenyl-N,N'-(1-naphthyl)-1,1'-biphenyl-4,4'-diamine, diphenylamine and N,N,N'-triphenylbenzidine, diphenylamine: N,N'-diphenylbenzidine is used to prepare organic long afterglow materials using a water matrix method, and the heating temperature in water is 55°C.

9. Application of organic long afterglow materials with multiple lifespans, colors and temperature stimulus responses in three-level encryption, characterized in that: The method comprises the preparation of an adhesive, using the adhesive to input information for the first time, and attaching and encrypting the information using the luminescent material prepared according to one of claims 5 to 8 as required.

10. Application of the organic long afterglow material with multiple lifespans, colors and temperature stimulus responses in three-level encryption according to claim 9, characterized in that: The adhesive is prepared by preparing a polyvinyl pyrrolidone aqueous solution.