Production method for improving lamellar tearing resistance of super-thick steel plate

By adopting one-stage rolling and two-stage water-cooling processes in the production of extra-thick steel plates, combined with specific chemical composition and treatment processes, the problems of insufficient layered tear resistance and high production costs of extra-thick steel plates are solved, and high efficiency is achieved. Low-cost steel plate production reduces mill losses and grain inhomogeneity.

CN119040590AActive Publication Date: 2024-11-29SD STEEL RIZHAO CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411000140.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-29
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

Extra-thick steel plates have shortcomings in their ability to resist layered tear. The existing production methods are costly, have long cycles and cause high loads to rolling mills and motors, resulting in shortening of losses and service life.

Method used

One-stage rolling is carried out using 300mm thick continuous casting billets, and the rolling is controlled to be completed in the complete recrystallization zone. It combines two-stage water-cooling process and specific chemical composition and treatment processes, including molten iron pretreatment, BOF steelmaking, LF refining, RH vacuum Treatment and pit cooling ensure that the steel plate is rolled and uniformly cooled in the fully recrystallized zone, reducing internal stress and grain inhomogeneity.

Benefits of technology

It improves the resistance to layered tear of extra-thick steel plates, reduces mill and motor losses, simplifies production processes, shortens cycles, reduces costs, and improves the low-temperature toughness and grain uniformity of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of super-thick steel plates, in particular to a production method for improving lamellar tearing resistance of a super-thick steel plate. According to the production method, a continuous casting billet with the thickness being 300 mm is adopted for first-stage rolling, the continuous casting billet is controlled to be rolled in a complete recrystallization area, the pass deformation rate xi meets the condition that 5 < = Trolling * xi / H < = 10, the unit of xi is%, Trolling represents the first-pass rolling temperature of the complete recrystallization area, H represents the thickness of a finished steel plate, and the sum of the deformation rates of at least one set of adjacent passes is not smaller than 30%; the steel plate is subjected to two-stage water cooling after being rolled, the surface temperature of the steel plate after first-stage water cooling is 600-650 DEG C, and the surface temperature of the steel plate after second-stage water cooling is 500-550 DEG C. The process is simple, the stability is high, the production period is short, the cost is low, the popularization and application prospects are wide, the low-temperature toughness of the product is excellent,-20 DEG C KV2 is larger than or equal to 110 J, and the percentage reduction of area is larger than or equal to 38%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of extra-thick steel plates, and in particular to a production method for improving the lamellar tearing resistance of extra-thick steel plates. Background Art

[0002] Thick and high-strength steel plates are widely used in wind power, high-rise buildings, offshore platforms, large venues and other fields that require high performance of steel plates. Due to the thickness of the plate, the resistance to lamellar tearing is poor. In order to improve the resistance of steel to lamellar tearing, the conventional practice is to use steel ingots for forging or composite casting to make the compression ratio>3, and then perform normalizing. The main disadvantages of this method are: ① The yield rate of steel ingots is low; ② The interface bonding strength of composite castings is poor, and the composite processing of castings is complex, the cost is high, and the metallurgical quality is not as high as that of continuous castings; ③ When using the normalizing process, a large amount of alloy elements need to be added to ensure strength, the production cost is high, and the welding process is complicated; ④ There are many production processes, long cycles, and high costs.

[0003] Chinese invention patent application CN 109897928 A uses continuous casting slabs with a thickness of 370~450nm, which are produced through high-cost smelting + strong electromagnetic stirring + high-energy heating + high-loss rolling + heat treatment. It has the disadvantages of large rolling mill losses, low yield, high cost, and long production cycle.

[0004] The continuous casting billet + TMCP process is currently widely used in the production of thin gauge steel plates, and the resulting products have the advantages of low alloy content, good metallurgical quality, low cost, and good welding performance. However, the application of this process in the field of thick, high-strength, and high-resistance lamellar tearing steel plates is difficult, especially under the conditions of a fixed continuous casting billet thickness and a low reduction ratio, there are obvious difficulties in using the TMCP short process to produce thick, high-strength, and high-resistance lamellar tearing steel plates.

[0005] Chinese invention patent application CN 116020867 A discloses a thermomechanical rolling method for improving the core performance of 80~100mm extra-thick high-strength and tough lamellar tear resistant steel plates. This method reduces the surface temperature of the billet by rapid water leakage in the high-temperature recrystallization zone during each rolling pass, thereby increasing the surface rolling deformation resistance and allowing the deformation to penetrate into the core. After multiple passes of repeated water leakage and high-pressure rolling, more complete recrystallization occurs in the core, promoting uniform phase change of the extra-thick steel plate, and obtaining excellent high-strength and toughness and lamellar tear resistance. The disadvantage of this method is that this process method requires high rolling mill rigidity and large motor torque, which causes the motor and steel rolling to work at high load or overload, increasing the loss of the rolling mill and motor and shortening the service life. Summary of the invention

[0006] In view of the problems that extra-thick steel plates have poor resistance to lamellar tearing, and the production cost and cycle of composite billets or steel ingots are high, the present invention provides a production method for improving the resistance to lamellar tearing of extra-thick steel plates, which is suitable for producing extra-thick steel plates with a thickness of 100-120 mm from 300 mm thick continuous casting billets. The present invention has simple process, high stability, short production cycle, low cost, great promotion and application prospects, and excellent low-temperature toughness of the product, KV2≥110J at -20℃, and cross-sectional shrinkage rate≥38%.

[0007] The technical solution of the present invention is as follows: A production method for improving the lamellar tear resistance of extra-thick steel plates, using a 300mm thick continuous casting billet for one-stage rolling, controlling the continuous casting billet to complete rolling in the complete recrystallization zone, and the pass deformation rate ξ satisfies 5≤T 轧 ×ξ / H≤10, the unit of ξ is %, where T 轧 Indicates the first rolling temperature in the complete recrystallization zone, i.e., the start rolling temperature, T 轧 =997+463×(%C)+890×(%Ti)+365×(%Al)+6137(%Nb)-641×(%Nb) 1 / 2 +742×(%V)-225×(%V) 1 / 2 , the unit is ℃; H represents the thickness of the finished steel plate, 100≤H≤120, the unit is mm; And the sum of deformation rates of at least one set of adjacent passes is not less than 30%; After rolling, the steel plate is water-cooled in two stages. After the first stage of water cooling, the surface temperature of the steel plate is 600~650℃, and after the second stage of water cooling, the surface temperature of the steel plate is 500~550℃.

[0008] Further, the chemical composition and weight percentage of the continuous casting slab are as follows: C 0.10%~0.14%, Si 0.20%~0.30%, Mn 1.70%~2.3%, P≤0.015%, S≤0.003%, Al0.020%~0.035%, 0.030%≤Nb+V+Ti≤0.070%, the balance is Fe and unavoidable impurities, and satisfies 0.40%≤C+Mn / 6≤0.46%.

[0009] Furthermore, the production method includes molten iron pretreatment → BOF steelmaking → LF refining → RH vacuum treatment → continuous casting → heating → rolling → water cooling → pit cooling.

[0010] Furthermore, after RH calcium treatment, the molten steel satisfies (%Ca)×(%S) 0.22 ≤2.5×10 -3On the one hand, it can further purify the molten steel, and on the other hand, it can modify the sulfides in the steel to make them non-deformable, stable and fine spherical sulfides, inhibit the hot brittleness of S, and improve the elongation and Z-direction properties of the rolled piece.

[0011] Furthermore, in order to avoid the harmful factors such as white spots and aluminum nitride that affect the plasticity of the material, it is necessary to reduce the nitrogen and hydrogen content, and the RH vacuum treatment is controlled to [H]×[N]≤3×10 -11 .

[0012] Furthermore, pit cooling is to put the water-cooled steel plate into a slow cooling pit for slow cooling, and control the steel plate entry temperature ≥350°C, slow cooling time ≥72h, and steel plate exit temperature ≤100°C. After vacuum treatment, the molten steel has low gas content, but hydrogen is absorbed during the heating process of the continuous casting billet. In order to allow the free hydrogen to fully escape after rolling, and to reduce the internal stress generated by the steel plate during the water cooling process, it is necessary to enter the pit for slow cooling to produce a "self-tempering" effect to release the internal stress.

[0013] Furthermore, the finished steel plate has a longitudinal KV2 of ≥110J at -20°C and a cross-sectional shrinkage of ≥38%.

[0014] The beneficial effects of the present invention are: (1) The present invention adopts a complete recrystallization zone rolling process, and the rolling deformation penetrates the interior of the rolled piece, and the internal grain size reaches 10 μm. In addition, the austenite recrystallization is fully utilized to uniformly form the grains in the thickness direction of the rolled piece, thereby solving the problem that the internal grains of extra-thick steel plates can only be refined by low temperature and high pressure reduction and the grain uniformity is poor. The losses of the rolling rollers, rolling mills, and motors are reduced, and the production efficiency is improved by one-stage rolling.

[0015] (2) The present invention adopts a two-stage water cooling process. In the first stage, water cooling causes a phase transformation to occur from the surface of the steel plate to 1 / 6 of the thickness, generating a ferrite + pearlite + a very small amount of bainite (5% to 8%) structure, and the ferrite grains are fine and uniform. In the second stage, water cooling increases the cooling intensity, causing a ferrite + pearlite phase transformation to occur from 1 / 6 of the thickness to the core of the steel plate, and the ferrite grains are uniform, reaching 10 μm as a whole; achieving high continuity of the full-thickness organizational type and high grain uniformity. DETAILED DESCRIPTION

[0016] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0017] The rolling process of the specific embodiment of the present invention is calculated according to the following formula: 轧 : T 轧 =997+463×(%C)+890×(%Ti)+365×(%Al)+6137×(%Nb)-641×(%Nb) 1 / 2 +742×(%V)-225×(%V) 1 / 2 , And the rolling process meets the following two conditions: ①5≤T 轧 ×ξ / H≤10, Where, ξ represents the deformation rate of the complete recrystallization zone, and the unit is %; H represents the thickness of the finished steel plate, 100≤H≤120, in mm; ② The sum of the deformation rates of at least one group of adjacent passes is not less than 30%, that is, the situation in which the sum of the deformation rates of two consecutive passes is not less than 30% occurs at least once. For example, in a rolling process, the sum of the deformation rates of the third pass and the fourth pass is not less than 30%, or, in a rolling process, the sum of the deformation rates of the second pass and the third pass is not less than 30% and the sum of the deformation rates of the third pass and the fourth pass is not less than 30%, and so on.

[0018] Example 1 A production method for improving the lamellar tearing resistance of extra-thick steel plates, comprising smelting (hot iron pretreatment → BOF steelmaking → LF refining → RH vacuum treatment) → continuous casting → heating → rolling → water cooling → pit cooling; Among them, the smelting process: using molten iron pretreatment, the final S content is 0.0025%; the converter adopts top and bottom double blowing, fully dephosphorized, the final phosphorus content is 0.004%, argon is blown throughout the process, weak stirring, the slag surface is slightly turned over without being exposed, and lime and fluorite are used to make white slag; the RH vacuum degree is 100pa, and the vacuum time is 15min; the molten steel is calmed for 40min before tapping, and calcium treatment (%Ca)×(%S) 0.22 =1.8×10 -3 , [H] × [N] = 2.8 × 10 -11 .

[0019] Continuous casting process: a continuous casting billet with a thickness of 300 mm is obtained. The chemical composition and weight percentage of the continuous casting billet are as follows: C 0.14%, Si 0.23%, Mn 1.78%, P 0.012%, S 0.001%, Al 0.032%, Nb 0.025%, V0.021%, Ti 0.018%, and the rest are Fe and inevitable impurities.

[0020] Heating process: Control the continuous casting billet outlet temperature to 1087℃.

[0021] Rolling process: The continuous casting billet is rolled after being descaled by 21MPa high-pressure water. One-stage rolling is adopted to control the continuous casting billet to complete rolling in the complete recrystallization zone. The rolling start temperature T is calculated according to the formula 轧 The rolling temperature is 1050℃, the sum of the deformation rates of the third and fourth passes is 38%, the cumulative deformation rate in the complete recrystallization zone is 60%, the final rolling temperature is 1018℃, and a steel plate with a thickness of 120mm is obtained.

[0022] Water cooling process: After rolling, the steel plate is subjected to two-stage water cooling. After the first stage of water cooling, the surface temperature of the steel plate is 640°C. After 90s, the second stage of water cooling is carried out. After the second stage of water cooling, the surface temperature of the steel plate is 530°C.

[0023] Pit cooling process: After water cooling, the steel plate enters the slow cooling pit for slow cooling. The slow cooling time is 80 hours. The temperature of the steel plate is 466°C when entering the pit, and 83°C when leaving the pit.

[0024] Example 2 A production method for improving the lamellar tearing resistance of extra-thick steel plates, comprising smelting (hot iron pretreatment → BOF steelmaking → LF refining → RH vacuum treatment) → continuous casting → heating → rolling → water cooling → pit cooling; Among them, the smelting process: using molten iron pretreatment, the final S content is 0.0023%; the converter adopts top and bottom double blowing, fully dephosphorized, the final phosphorus content is 0.005%, argon is blown throughout the process, weak stirring, the slag surface is slightly turned over without being exposed, and lime and fluorite are used to make white slag; the RH vacuum degree is 100pa, and the vacuum time is 14min; the molten steel is calmed for 38min before tapping, and calcium treatment (%Ca)×(%S) 0.22 =2.0×10 -3 , [H] × [N] = 2.8 × 10 -11 .

[0025] Continuous casting process: a continuous casting billet with a thickness of 300 mm is obtained. The chemical composition and weight percentage of the continuous casting billet are as follows: C 0.10%, Si 0.24%, Mn 2.05%, P 0.013%, S 0.002%, Al 0.029%, Nb 0.022%, V0.023%, Ti 0.018%, and the rest are Fe and inevitable impurities.

[0026] Heating process: Control the continuous casting billet outlet temperature to 1067℃.

[0027] Rolling process: The continuous casting billet is rolled after being descaled by 21MPa high-pressure water. One-stage rolling is adopted to control the continuous casting billet to complete rolling in the complete recrystallization zone. The rolling start temperature T is calculated according to the formula轧 The temperature is 998℃, the sum of the deformation rates of the third and fourth passes is 43%, the cumulative deformation rate in the complete recrystallization zone is 73.33%, the final rolling temperature is 958℃, and a steel plate with a thickness of 100mm is obtained.

[0028] Water cooling process: After rolling, the steel plate is subjected to two-stage water cooling. After the first stage of water cooling, the surface temperature of the steel plate is 628°C. The second stage of water cooling is carried out after 67s. After the second stage of water cooling, the surface temperature of the steel plate is 542°C.

[0029] Pit cooling process: After water cooling, the steel plate enters the slow cooling pit for slow cooling. The slow cooling time is 73h. The temperature of the steel plate is 446℃ when entering the pit, and 84℃ when leaving the pit.

[0030] The properties of the steel plates prepared in Example 1 and Example 2 were tested, and the results are shown in Table 1.

[0031] Table 1 Properties of the steel plates of Example 1 and Example 2 of the present invention

[0032] Although the present invention has been described in detail by way of preferred embodiments, the present invention is not limited thereto. Without departing from the spirit and essence of the present invention, a person of ordinary skill in the art may make various equivalent modifications or substitutions to the embodiments of the present invention, and such modifications or substitutions shall be within the scope of the present invention. Any person of ordinary skill in the art may easily conceive of changes or substitutions within the technical scope disclosed by the present invention, and such changes or substitutions shall be within the scope of protection of the present invention.

Claims

1. A production method for improving the lamellar tearing resistance of extra-thick steel plates, characterized in that: The continuous casting billet with a thickness of 300 mm is used for one-stage rolling. The continuous casting billet is controlled to complete rolling in the complete recrystallization zone, and the pass deformation rate ξ satisfies 5≤T 轧 ×ξ / H≤10, the unit of ξ is %, where T 轧 Indicates the first rolling temperature in the complete recrystallization zone, i.e., the start rolling temperature, T 轧 =997+463×(%C)+890×(%Ti)+365×(%Al)+6137×(%Nb)-641×(%Nb) 1 / 2 +742×(%V)-225×(%V) 1 / 2 , the unit is ℃; H represents the thickness of the finished steel plate, 100≤H≤120, the unit is mm; And the sum of deformation rates of at least one set of adjacent passes is not less than 30%; After rolling, the steel plate is water-cooled in two stages. After the first stage of water cooling, the surface temperature of the steel plate is 600~650℃, and after the second stage of water cooling, the surface temperature of the steel plate is 500~550℃.

2. The production method according to claim 1, characterized in that The chemical composition and weight percentage of the continuous casting billet are as follows: C 0.10%~0.14%, Si 0.20%~0.30%, Mn 1.70%~2.3%, P≤0.015%, S≤0.003%, Al 0.020%~0.035%, 0.030%≤Nb+V+Ti≤0.070%, the balance is Fe and unavoidable impurities, and satisfies 0.40%≤C+Mn / 6≤0.46%.

3. The production method according to claim 1, characterized in that The production method includes molten iron pretreatment → BOF steelmaking → LF refining → RH vacuum treatment → continuous casting → heating → rolling → water cooling → pit cooling.

4. The production method according to claim 3, characterized in that After RH calcium treatment, the molten steel meets (%Ca)×(%S) 0.22 ≤2.5×10 -3 .

5. The production method according to claim 3, characterized in that RH vacuum treatment control [H] × [N] ≤ 3 × 10 -11 .

6. The production method according to claim 3, characterized in that Pit cooling is to put the water-cooled steel plate into a slow cooling pit for slow cooling, control the steel plate entering the pit temperature ≥350℃, slow cooling time ≥72h, and the steel plate exiting the pit temperature ≤100℃.

7. The production method according to claim 1, characterized in that The -20℃ longitudinal KV2 of the finished steel plate is ≥110J.

8. The production method according to claim 1, characterized in that The cross-sectional shrinkage of the finished steel plate is ≥38%.

Citation Information

Patent Citations

  • Low-compression-ratio large-thickness laminar tearing resistant steel plate and manufacturing method thereof

    CN111748678A

  • Super-thick steel plate with excellent core low-temperature impact toughness and manufacturing method of super-thick steel plate

    CN115094316A

  • Thermal mechanical rolling method for improving core performance of 80-100mm extra-thick high-toughness lamellar-tearing-resistant steel plate

    CN116020867A

  • Extra-thick plate and preparation method thereof

    CN117165849A

  • Method for rolling steel plate

    CN117920747A