650 DEG C grade ferronickel-based high-temperature alloy boiler tube fusion welding joint and preparation and heat treatment method thereof
Through solid solution heat treatment before welding and stress removal heat treatment after welding, the thermal cracking and residual stress problems during the welding process of nickel-iron-based high-temperature alloy boiler pipes are solved, the stability and high-temperature performance of the welded joints are improved, and the service life of the boiler pipes is extended .
Patent Information
- Application Number
- CN202411160624.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-29
AI Technical Summary
During the welding process, the weld metal and welding heat-affected zone have a high tendency to crack. After the welding thermal cycle, the joints produce a large amount of shrinkage, deformation and residual stress, resulting in poor durability and fatigue performance of high-temperature components.
The boiler tube is subjected to solid solution heat treatment before welding, and the solid solution reinforced nickel-based high-temperature alloy is used as the welding material. It is welded by tungsten argon arc welding, and the stress-removing heat treatment is carried out at 750-800℃, and the temperature is slowly raised and the heat is insulated to release. Residual stress.
Effectively adjust the microstructure of the material, eliminate residual stress and non-equilibrium structure, improve the stability and reliability of welded joints, extend the service life of boiler pipes, reduce the tendency of thermal cracking and stress concentration of welded joints, improve the performance and Security.
Smart Images

Figure CN119040613A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of heat treatment, and in particular relates to a 650°C grade nickel-iron-based high-temperature alloy boiler tube fusion welding joint and a preparation and heat treatment method thereof. Background Art
[0002] Under the dual pressures of global energy structure transformation and environmental protection, the power industry is developing in a more efficient and environmentally friendly direction. Coal-fired power technology of 650℃ and above is the main push direction of the power industry. It is one of the effective ways to achieve industrial upgrading and standardization of my country's power industry to achieve high efficiency, low fuel consumption and low emissions in a relatively short period of time. Compared with ultra-supercritical units, raising its steam temperature parameters to 650℃ puts more stringent requirements on the structural stability of the unit's high-temperature components and the reliability of welded joints. Among them, the boiler tube is one of the core components with the most stringent service environment of the entire unit, and its manufacturing material is planned to be nickel-based / nickel-iron-based high-temperature alloy.
[0003] At present, nickel-based / nickel-iron-based high-temperature alloys are being considered as materials for the manufacture of boiler tubes due to their excellent high-temperature performance and oxidation resistance. However, due to their high thermal expansion coefficient and low thermal conductivity, the weld metal and the heat-affected zone have a high tendency to thermal cracking during welding; and after undergoing welding thermal cycles, a large amount of shrinkage, deformation and residual stress will be generated in the formed joints, which have a great impact on the durability and fatigue properties of high-temperature components.
[0004] During the welding process of nickel-iron-based high-temperature alloys, the weld metal and the welding heat-affected zone have a high tendency to thermal cracking. After the welding thermal cycle, a large amount of shrinkage, deformation and residual stress will be generated in the joint, resulting in poor durability and fatigue performance of high-temperature components. It is particularly important to find a new high-temperature alloy welding method and joint post-weld treatment process. Summary of the invention
[0005] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a 650°C grade nickel-iron-based high-temperature alloy boiler tube fusion-welded joint and its preparation and heat treatment method, so as to solve the technical problems that the weld metal and the welding heat-affected zone of the existing nickel-iron-based high-temperature alloy boiler tube fusion-welded joint have a large tendency to thermal cracking during the welding process, and the joint will produce a large amount of shrinkage, deformation and residual stress after the welding thermal cycle.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] The invention discloses a method for preparing a 650°C grade nickel-iron-based high-temperature alloy boiler tube fusion welding joint, comprising: firstly performing a pre-welding solid solution heat treatment on the boiler tube, and then welding the boiler tube with a welding material to obtain a 650°C grade nickel-iron-based high-temperature alloy boiler tube fusion welding joint;
[0008] The material of the boiler tube is a precipitation-strengthened nickel-iron-based high-temperature alloy; the material of the welding material is a solid solution-strengthened nickel-based high-temperature alloy.
[0009] Preferably, the precipitation-strengthened nickel-iron-based high-temperature alloy includes, in mass percentage, Fe: 28%-32%, Cr: 16%-20%, Ti: 1.5%-2.5%, Al: 1.3%-2.0%, W: 0.1%-0.5%, Si: 0.1%-0.5%, C: 0.05%-0.08%, Zr: 0.01%-0.05%, B: 0.003%-0.006%, and the rest is Ni.
[0010] Preferably, in terms of mass percentage, Fe+Ni>50%.
[0011] Preferably, in terms of mass percentage, Al+Ti≥3.0%.
[0012] Preferably, the strengthening phase of the precipitation-strengthened nickel-iron-based high-temperature alloy is mainly γ'-Ni3(Al,Ti).
[0013] Preferably, the welding method is argon tungsten arc welding.
[0014] Preferably, the boiler tube is in a solid solution state after being subjected to solution heat treatment before welding; the material of the boiler tube is strongly matched with the welding material.
[0015] Preferably, the temperature of the pre-welding solution heat treatment of the boiler tube is 1000-1160° C. and the time is 0.5-2 h.
[0016] The invention also discloses a 650°C grade nickel-iron-based high-temperature alloy boiler tube fusion welding joint obtained by the preparation method.
[0017] The present invention also discloses a heat treatment method for the above-mentioned 650°C grade nickel-iron-based high-temperature alloy boiler tube fusion welding joint, which performs stress relief heat treatment on the 650°C grade nickel-iron-based high-temperature alloy boiler tube fusion welding joint at a heating rate of 1-5°C / min and keeping the temperature at 750-800°C for 1-4h.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] The invention discloses a preparation method of a 650°C grade nickel-iron-based high-temperature alloy boiler tube fusion welding joint. The method comprises the following steps: firstly performing a pre-welding solid solution heat treatment on a boiler tube made of a precipitation-strengthened nickel-iron-based high-temperature alloy, so as to effectively adjust the microstructure of the material, eliminate residual stress and unbalanced structure in the boiler tube, improve the plasticity and toughness of the material, and make the subsequent welding process more stable and reliable. The precipitation-strengthened nickel-iron-based high-temperature alloy has good high-temperature performance and oxidation resistance, can meet the use requirements in high-temperature environments such as high-parameter ultra-supercritical thermal power units, ensure that the boiler tube can work stably at high temperatures, and extend the service life. Then, the boiler tube is welded with welding materials made of solid solution strengthened nickel-based high-temperature alloy to obtain a 650°C grade nickel-iron-based high-temperature alloy boiler tube fusion welding joint; the solid solution strengthened nickel-based high-temperature alloy is used as the welding material. Since the solid solution strengthened alloy usually has better plasticity and toughness, it can better adapt to the thermal stress and mechanical stress in the welding process. When welding with the boiler tube of precipitation strengthened nickel-iron-based high-temperature alloy, the weld metal of the solid solution strengthened nickel-based high-temperature alloy can reduce the tendency of hot cracks in the joint during welding, and is not prone to organizational transformation, which is conducive to maintaining the stability and reliability of the welded joint.
[0020] Furthermore, the performance of precipitation-strengthened nickel-iron-based high-temperature alloys can be optimized by precisely controlling the content of alloying elements. For example, the content of elements such as Fe and Cr has an important influence on the corrosion resistance and oxidation resistance of the alloy; Ti and Al are the main forming elements of the γ' phase and play a key role in the high-temperature strength of the alloy; while elements such as C and B help to refine the grains and improve the strength and toughness of the alloy.
[0021] Furthermore, keeping the total amount of Fe+Ni above 50% can ensure the basic performance and structural stability of the alloy. Al and Ti are the main forming elements of the γ' phase. Increasing the content of Al+Ti can promote the precipitation of the γ' phase, thereby improving the high temperature strength and creep resistance of the alloy. The γ' phase is a stable precipitation phase, which can effectively improve the high temperature strength of the alloy. Ensuring that the γ' phase is the main strengthening phase can significantly improve the performance of the alloy.
[0022] Furthermore, argon tungsten arc welding is a high-quality welding method that can achieve high-quality welding under a protective atmosphere, reduce welding defects, and improve the performance of welded joints.
[0023] Furthermore, after the pre-welding solid solution heat treatment, the boiler tube is in a solid solution state, which is beneficial to the subsequent welding process. At the same time, the equal strength matching of the boiler tube and the welding material can ensure that the performance of the welded joint is similar to that of the parent material, thus improving the overall performance.
[0024] Furthermore, selecting the appropriate solution heat treatment temperature and time before welding can ensure that the alloy elements in the boiler tube are fully dissolved to form a uniform solid solution, providing good conditions for the subsequent welding process. At the same time, it can also avoid grain growth and performance degradation caused by excessively high temperatures and excessively long times.
[0025] The present invention also discloses a 650°C grade nickel-iron-based high-temperature alloy boiler tube fusion welding joint obtained by the above-mentioned preparation method, which can meet the high-temperature working environment requirements at the 650°C level, and when used in a high-temperature environment such as an ultra-supercritical thermal power unit, can maintain stable performance and improve the safety and reliability of the entire system.
[0026] The present invention also discloses a heat treatment method for the above-mentioned 650°C grade nickel-iron-based high-temperature alloy boiler tube fusion welding joint, which performs stress relief heat treatment on the 650°C grade nickel-iron-based high-temperature alloy boiler tube fusion welding joint at a heating rate of 1-5°C / min and is kept at 750-800°C for 1-4h. The slow heating rate helps to reduce the thermal stress and deformation generated in the welded joint during the heat treatment process and maintain the shape and dimensional stability of the joint. Appropriate temperature and holding time can ensure that the residual stress in the welded joint is effectively released while avoiding adverse effects on material properties. Stress relief heat treatment can eliminate the residual stress generated during the welding process, improve the fatigue life and service safety of the welded joint, and effectively reduce the risk of cracking of the welded joint due to stress concentration during use. Aiming at the service requirements of key high-temperature components of high-parameter (650℃) ultra-supercritical thermal power units, and combining the processing characteristics of nickel-iron-based high-temperature alloys, effective post-weld treatment can be used to regulate the organization and relieve stress, thereby improving the quality and reliability of welded joints, effectively reducing the thermal cracking tendency of weld metal, and reducing the welding residual stress of joints. The stress relaxation test results of welded joints at 780℃ showed that the initial loading force was 5914N. After about 4h, the loading force was reduced to 3002N, a decrease of about 50%. After 10h, the loading force was further reduced to 2567N, a decrease of about 60%, which improved the service safety of high-temperature components of nickel-based / nickel-iron-based high-temperature alloy superheater tube screens. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a structural schematic diagram of a 650°C grade nickel-iron-based high-temperature alloy boiler tube fusion welding joint disclosed in the present invention;
[0028] Figure 2 It is a schematic diagram of the post-weld heat treatment process of the 650°C grade nickel-iron-based high-temperature alloy boiler tube fusion welding joint disclosed in the present invention;
[0029] Figure 3The stress relaxation test result of the 650°C grade nickel-iron-based high-temperature alloy boiler tube fusion welded joint disclosed in Example 3 of the present invention at 780°C is performed on the welded joint;
[0030] Figure 4 The microstructure photograph of the welded joint of the 650°C grade nickel-iron-based high-temperature alloy boiler tube fusion welded joint disclosed in Example 3 of the present invention; wherein (a) is the base material; (b) is the fusion line area; (c) is the base weld metal; (d) is the cap weld metal;
[0031] Figure 5 This is a microstructure photograph of the welded joint of the 650°C grade nickel-iron-based high-temperature alloy boiler tube fusion welded joint disclosed in Example 3 of the present invention, which was heat treated at 780°C for 4 hours after welding: wherein, (a) is the base material; (b) is the fusion line area; (c) is the base weld metal; and (d) is the cover weld metal. DETAILED DESCRIPTION
[0032] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0033] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0034] The present invention is further described in detail below in conjunction with the accompanying drawings:
[0035] See also Figure 1 The present invention discloses a 650°C grade nickel-iron-based high-temperature alloy boiler tube fusion welding joint. As can be seen from the figure, the 650°C grade nickel-iron-based high-temperature alloy boiler tube fusion welding joint includes boiler tubes made of precipitation-strengthened nickel-iron-based high-temperature alloy at both ends, and an intermediate welding material made of solid solution-strengthened nickel-based high-temperature alloy.
[0036] See also Figure 2 The figure is a schematic diagram of the post-weld heat treatment process of the 650°C grade nickel-iron-based high-temperature alloy boiler tube fusion welding joint disclosed in the present invention; it can be seen from the figure that during the post-weld heat treatment, the temperature is raised to 750-800°C at a rate of 1-5°C / min, kept warm for 1-4h, and then slowly cooled to room temperature with the furnace.
[0037] See also Figure 3 The stress relaxation test results of the 650°C grade nickel-iron-based high-temperature alloy boiler tube fusion welding joint disclosed in Example 3 of the present invention were carried out at 780°C. As can be seen from the figure, the initial loading force is 5914N. After about 4 hours, the loading force is reduced to 3002N, a decrease of about 50%. After 10 hours, the loading force is reduced to 2567N, a decrease of about 60%.
[0038] See also Figure 4 The microstructure photograph of the welded joint of the 650°C grade nickel-iron-based high-temperature alloy boiler tube fusion welded joint disclosed in Example 3 of the present invention; wherein (a) is the base material; (b) is the fusion line area; (c) is the base weld metal; (d) is the cap weld metal; Figure 5 This is a microstructure photo of the welded joint of the 650℃ grade nickel-iron-based high-temperature alloy boiler tube fusion welded joint disclosed in Example 3 of the present invention after heat treatment at 780℃ for 4h after welding: (a) is the base material; (b) is the fusion line area; (c) is the base weld metal; (d) is the cap weld metal. Figure 4 and Figure 5 It can be seen that the microstructure of the weld metal of the weld joint in the as-welded state and the state after post-weld heat treatment is not much different, both of which are austenitic structures.
[0039] The invention discloses a 650°C grade nickel-iron-based high-temperature alloy boiler tube fusion welding joint, comprising a boiler tube and a welding material connected to the boiler tube; wherein the material of the boiler tube is a precipitation-strengthened nickel-iron-based high-temperature alloy, the welding material is a solid solution-strengthened nickel-based high-temperature alloy, the boiler tube is connected to the welding material by a fusion welding method, and a post-weld stress relief heat treatment is performed on the formed joint to relieve welding residual stress.
[0040] Preferably, in terms of mass percentage, the composition (mass fraction, wt.%) of the precipitation-strengthened nickel-iron-based high-temperature alloy satisfies Fe: 28%-32%, Cr: 16%-20%, Ti: 1.5%-2.5%, Al: 1.3%-2.0%, W: 0.1%-0.5%, Si: 0.1%-0.5%, C: 0.05%-0.08%, Zr: 0.01%-0.05%, B: 0.003%-0.006%, and the remainder is Ni; wherein the mass percentage of Fe+Ni is greater than 50%, and the mass percentage of Al+Ti is greater than or equal to 3.0%.
[0041] Preferably, the welding material is a solid solution strengthened nickel-based high temperature alloy.
[0042] The present invention discloses a method for preparing a 650°C grade nickel-iron-based high-temperature alloy boiler tube fusion welding joint and a post-weld heat treatment method thereof, comprising:
[0043] Step 1: Perform solution heat treatment on the boiler tube before welding at a temperature of 1000-1160°C for a holding time of 0.5-2h, and match the welding materials;
[0044] Step 2, using welding materials to connect boiler tubes to obtain 650° C. grade nickel-iron-based high-temperature alloy boiler tube fusion welding joints;
[0045] Step 3, performing stress relief heat treatment on the 650°C grade nickel-iron-based high-temperature alloy boiler tube fusion welding joint.
[0046] Preferably, in step 1, the treatment state of the nickel-iron based alloy before welding is a solid solution state, and the principle of selecting the welding material is close to equal strength matching.
[0047] Preferably, in step 1, the boiler tube material is a precipitation-strengthened nickel-iron-based high-temperature alloy, and the selected welding material is a solid solution-strengthened nickel-based high-temperature alloy.
[0048] Preferably, in step 3, the stress relief heat treatment process is: heating to 750-800°C at a rate of 1-5°C / min, keeping the temperature for 1-4h, and then slowly cooling to room temperature in the furnace.
[0049] Example 1
[0050] A preparation method and joint heat treatment method of a 650℃ grade nickel-iron-based high-temperature alloy boiler tube fusion welding joint, comprising: firstly heat treating a precipitation-strengthened nickel-iron-based high-temperature alloy boiler tube at 1160℃ for 0.5h, then connecting the boiler tube with a solid solution-strengthened nickel-iron-based high-temperature alloy welding material to obtain a 650℃ grade nickel-iron-based high-temperature alloy boiler tube fusion welding joint; finally, performing stress relief heat treatment and cooling to room temperature. The chemical composition (mass fraction, wt.%) of the parent material precipitation-strengthened nickel-iron-based high-temperature alloy is Fe: 30%, Cr: 19%, Ti: 1.8%, Al: 1.8%, W: 0.3%, Si: 0.1%, C: 0.07%, Zr: 0.02%, B: 0.005%, and the balance is Ni; wherein the mass percentage of Fe+Ni is about 77%, and the mass percentage of Al+Ti is 3.6%. The welding material grade is ERNiCrCoMo-1 solid solution-strengthened nickel-based alloy, and the welding method is tungsten inert gas arc. After welding, heat the furnace to 750℃ at 3℃ / min, keep it at that temperature for 2h, and cool it to room temperature.
[0051] Example 2
[0052] A preparation method and joint heat treatment method of a 650℃ grade nickel-iron-based high-temperature alloy boiler tube fusion welding joint, comprising: firstly heat treating a precipitation-strengthened nickel-iron-based high-temperature alloy boiler tube at 1120℃ for 1h, then connecting the boiler tube with a solid solution-strengthened nickel-iron-based high-temperature alloy welding material to obtain a 650℃ grade nickel-iron-based high-temperature alloy boiler tube fusion welding joint, and finally performing stress relief heat treatment and cooling to room temperature. The chemical composition (mass fraction, wt.%) of the parent material precipitation-strengthened nickel-iron-based high-temperature alloy is Fe: 30%, Cr: 19%, Ti: 1.8%, Al: 1.8%, W: 0.3%, Si: 0.1%, C: 0.07%, Zr: 0.02%, B: 0.005%, and the balance is Ni; wherein the mass percentage of Fe+Ni is about 77%, and the mass percentage of Al+Ti is 3.6%. The welding material grade is ERNiCrCoMo-1 solid solution-strengthened nickel-based alloy, and the welding method is tungsten inert gas arc welding.
[0053] After welding is completed, the furnace temperature is raised to 780°C at 3°C / min, kept at this temperature for 2 hours, and then cooled to room temperature.
[0054] Example 3
[0055] A preparation method and joint heat treatment method of a 650℃ grade nickel-iron-based high-temperature alloy boiler tube fusion welding joint, comprising: firstly heat treating a precipitation-strengthened nickel-iron-based high-temperature alloy boiler tube at 1100℃ for 1h, then connecting the boiler tube with a solid solution-strengthened nickel-iron-based high-temperature alloy welding material to obtain a 650℃ grade nickel-iron-based high-temperature alloy boiler tube fusion welding joint, and finally performing stress relief heat treatment and cooling to room temperature. The chemical composition (mass fraction, wt.%) of the parent material precipitation-strengthened nickel-iron-based high-temperature alloy is Fe: 30%, Cr: 19%, Ti: 1.8%, Al: 1.8%, W: 0.3%, Si: 0.1%, C: 0.07%, Zr: 0.02%, B: 0.005%, and the balance is Ni; wherein the mass percentage of Fe+Ni is about 77%, and the mass percentage of Al+Ti is 3.6%. The welding material grade is ERNiCrCoMo-1 solid solution-strengthened nickel-based alloy, and the welding method is tungsten inert gas arc welding.
[0056] After welding is completed, the furnace temperature is raised to 780°C at 3°C / min, kept at this temperature for 4 hours, and then cooled to room temperature.
[0057] Example 4
[0058] A preparation method and joint heat treatment method of a 650℃ grade nickel-iron-based high-temperature alloy boiler tube fusion welding joint, comprising: firstly heat treating a precipitation-strengthened nickel-iron-based high-temperature alloy boiler tube at 1060℃ for 1h, then connecting the boiler tube with a solid solution-strengthened nickel-iron-based high-temperature alloy welding material to obtain a 650℃ grade nickel-iron-based high-temperature alloy boiler tube fusion welding joint, and finally performing stress relief heat treatment and cooling to room temperature. The chemical composition (mass fraction, wt.%) of the parent material precipitation-strengthened nickel-iron-based high-temperature alloy is Fe: 28%, Cr: 20%, Ti: 1.5%, Al: 2.0%, W: 0.1%, Si: 0.5%, C: 0.05%, Zr: 0.05%, B: 0.003%, and the balance is Ni; wherein the mass percentage of Fe+Ni is about 76%, and the mass percentage of Al+Ti is 3.5%. The welding material grade is ERNiCrCoMo-1 solid solution-strengthened nickel-based alloy, and the welding method is tungsten inert gas arc welding.
[0059] After welding is completed, the furnace temperature is raised to 750°C at 3°C / min, kept at this temperature for 3 hours, and then cooled to room temperature.
[0060] Example 5
[0061] A preparation method and joint heat treatment method of a 650℃ grade nickel-iron-based high-temperature alloy boiler tube fusion welding joint, comprising: firstly heat treating a precipitation-strengthened nickel-iron-based high-temperature alloy boiler tube at 1000℃ for 2h, then connecting the boiler tube with a solid solution-strengthened nickel-iron-based high-temperature alloy welding material to obtain a 650℃ grade nickel-iron-based high-temperature alloy boiler tube fusion welding joint, and finally performing stress relief heat treatment and cooling to room temperature. The chemical composition (mass fraction, wt.%) of the parent material precipitation-strengthened high-temperature alloy is Fe: 32%, Cr: 16%, Ti: 2.5%, Al: 1.3%, W: 0.5%, Si: 0.1%, C: 0.08%, Zr: 0.01%, B: 0.006%, and the balance is Ni; the mass percentage of Fe+Ni is about 80%, and the mass percentage of Al+Ti is 3.8%. The welding material grade is ERNiCrCoMo-1 solid solution-strengthened nickel-based alloy, and the welding method is tungsten inert gas arc welding.
[0062] After welding is completed, the furnace temperature is raised to 800°C at 3°C / min, kept at this temperature for 1 hour, and then cooled to room temperature.
[0063] The present invention discloses a 650°C grade nickel-iron-based high-temperature alloy boiler tube fusion welding joint and a preparation method and a heat treatment method thereof. Aiming at the service requirements of key high-temperature components of high-parameter (650°C) ultra-supercritical thermal power units, and combining the processing characteristics of nickel-iron-based high-temperature alloys, effective post-weld treatment can be used to regulate the structure and relieve stress, thereby improving the quality and reliability of the welded joint, effectively reducing the thermal cracking tendency of the weld metal, and reducing the welding residual stress of the joint. Figure 3 As shown in the stress relaxation test results of the welded joint at 780°C, the initial loading force is 5914N. After about 4 hours, the loading force is reduced to 3002N, a decrease of about 50%. After 10 hours, the loading force is further reduced to 2567N, a decrease of about 60%, thereby improving the service safety of the high-temperature components of the nickel-based / nickel-iron-based high-temperature alloy superheater tube screen. The boiler tube connection of the present invention is a structural welding of dissimilar high-temperature alloys. The solid solution-strengthened nickel-based alloy welding material is used to connect the precipitation-strengthened nickel-iron-based alloy, and then the formed joint is subjected to post-weld heat treatment. The advantages are that the welding quality control of the high-temperature alloy joint is: (1) The solid solution-strengthened nickel-based alloy weld metal can reduce the tendency of the joint to produce thermal cracks during welding; (2) The post-weld heat treatment will not cause obvious structural changes in the weld metal. The weld metal is a solid solution-strengthened high-temperature alloy. By comparing the microstructure photos of the joint in the welded state and before and after heat treatment, as shown in FIG. Figure 4 and Figure 5 As shown in the figure, it was found that the weld metal was all austenite without obvious structural changes; (3) Slow cooling in the furnace after heat treatment will relieve the residual stress in the dissimilar joints. According to the stress relaxation test of the welded joint, it can be proved that the residual stress level in the joint decreases after heat treatment.
[0064] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. A method for preparing a 650°C grade nickel-iron-based high-temperature alloy boiler tube fusion welding joint, characterized in that: include: Firstly, the boiler tube is subjected to solution heat treatment before welding, and then the boiler tube is welded with welding materials to obtain a 650℃ grade nickel-iron-based high-temperature alloy boiler tube fusion welding joint; The material of the boiler tube is a precipitation-strengthened nickel-iron-based high-temperature alloy; the material of the welding material is a solid solution-strengthened nickel-based high-temperature alloy.
2. The method for preparing a 650°C grade nickel-iron-based high-temperature alloy boiler tube fusion welding joint according to claim 1, characterized in that: The precipitation-strengthened nickel-iron-based high-temperature alloy comprises, by mass percentage, 28%-32% Fe, 16%-20% Cr, 1.5%-2.5% Ti, 1.3%-2.0% Al, 0.1%-0.5% W, 0.1%-0.5% Si, 0.05%-0.08% C, 0.01%-0.05% Zr, 0.003%-0.006% B, and the remainder is Ni.
3. The method for preparing a 650°C grade nickel-iron-based high-temperature alloy boiler tube fusion welding joint according to claim 2, characterized in that: In terms of mass percentage, the Fe+Ni>50%.
4. The method for preparing a 650°C grade nickel-iron-based high-temperature alloy boiler tube fusion welding joint according to claim 2, characterized in that: In terms of mass percentage, the Al+Ti≥3.0%.
5. The method for preparing a 650°C grade nickel-iron-based high-temperature alloy boiler tube fusion welding joint according to claim 1, characterized in that: The strengthening phase of the precipitation-strengthened nickel-iron-based high-temperature alloy is mainly γ'-Ni3(Al,Ti).
6. The method for preparing a 650°C grade nickel-iron-based high-temperature alloy boiler tube fusion welding joint according to claim 1, characterized in that: The welding method is tungsten inert gas arc welding.
7. The method for preparing a 650°C grade nickel-iron-based high-temperature alloy boiler tube fusion welding joint according to claim 1, characterized in that: The boiler tube is in a solid solution state after being subjected to solution heat treatment before welding; the material of the boiler tube is strongly matched with the welding material.
8. The method for preparing a 650°C grade nickel-iron-based high-temperature alloy boiler tube fusion welding joint according to claim 1, characterized in that: The temperature of the pre-welding solution heat treatment of the boiler tube is 1000-1160° C. and the time is 0.5-2 hours.
9. A 650°C grade nickel-iron-based high-temperature alloy boiler tube fusion welded joint obtained by the preparation method according to any one of claims 1 to 8.
10. The heat treatment method of 650°C grade nickel-iron-based high temperature alloy boiler tube fusion welding joint according to claim 9, characterized in that: The stress relief heat treatment of 650℃ grade nickel-iron-based high-temperature alloy boiler tube fusion welding joints was carried out at 750-800℃ for 1-4h at a heating rate of 1-5℃ / min.
Citation Information
Patent Citations
Rotor for steam turbine with temperature of 650 DEG C and above and preparation method of rotor
CN115044818A
Header for boiler unit with temperature of 650 DEG C and above and preparation method of header
CN115198161A
Preparation method of stop valve for boiler of unit at temperature of 650 DEG C or above
CN117102814A
METHOD OF PRODUCING Ni-BASED HEAT-RESISTANT ALLOY WELD JOINT, AND WELD JOINT PRODUCED BY THE METHOD
JP2016000414A
High-temperature nickel-based alloy for 700°c grade ultra-supercritical coal-fired power station and preparation thereof
WO2015123918A1