Method for modifying vanadium slag before vanadium extraction and tapping of molten iron converter

Through the special slag mixing agent, the FeO content is adjusted according to the content of silicon molten iron, and the physical properties of the slag are changed, and the problem of thin vanadium slag in the high silicon content is solved, thus achieving the effect of reducing oxidation and fluidity and improving vanadium recovery.

CN119040663AActive Publication Date: 2024-11-29PANZHIHUA HENG HAO CASTING CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411164092.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

During the vanadium extraction process, the high silicon content of molten iron causes the vanadium slag to be too thin and have good fluidity, resulting in serious slag roll when semi-steel is discharged. The existing technology is difficult to effectively reduce vanadium slag loss and maintain the vanadium slag grade.

Method used

The special slag mixing agent is used, which consists of 80% carbonaceous material, 12-17% aluminum-containing slag-forming material and 3-8% binder. The amount of slag mixing agent is adjusted according to the content of silicon molten iron, and the FeO content is controlled to change. The melting point and viscosity of the slag reduce oxidation and fluidity.

Benefits of technology

It significantly reduces the oxidation of vanadium slag, increases the viscosity of the slag, reduces the fluidity, reduces the slag roll when half-steel is discharged, and improves the vanadium recovery rate and vanadium extraction efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040663A_ABST
    Figure CN119040663A_ABST
Patent Text Reader

Abstract

The invention discloses a method for modifying vanadium slag before molten iron converter vanadium extraction and tapping, and belongs to the technical field of metallurgy. In order to solve the problems in the existing converter vanadium extraction process, the invention provides a method for modifying vanadium slag before molten iron converter vanadium extraction and tapping, which comprises the following steps of: after oxygen blowing of a vanadium extraction converter is finished, adding different amounts of slag modifier according to the silicon content in molten iron; when the silicon content of the molten iron is less than 0.18 wt%, the slag modifier is not added; when the silicon content of the molten iron is 0.18-0.21 wt%, adding 1.5-2.5 kg of slag modifier per ton of semisteel; when the silicon content of the molten iron is larger than 0.21 wt%, 2.5-3 kg of slag modifier is added per ton of semisteel; the slag modifier is composed of a carbonaceous material, an aluminum-containing slagging material and a binder. By adding the special slag modifier and strictly controlling the adding indexes of the slag modifier, the oxidability of the vanadium slag can be effectively reduced, the viscosity of the slag is increased, the fluidity is reduced, the slag entrapment amount during tapping is reduced, and the vanadium slag loss is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallurgy, and in particular relates to a method for modifying vanadium slag before vanadium extraction and steelmaking in a molten iron converter. Background Art

[0002] When the silicon content of vanadium-titanium molten iron is high (silicon content is greater than 0.18%), the slag at the end of vanadium extraction becomes very thin. The vanadium slag at the end of vanadium extraction has good fluidity. When the semi-steel tapping speed is relatively fast, it will inevitably cause serious slag rolling, resulting in serious loss of vanadium slag during the semi-steel tapping process. Other conventional means of increasing slag viscosity, such as adding lime and silica, cannot be used because they will reduce the grade of vanadium slag. Therefore, it is necessary to reduce the oxidation of vanadium slag from the perspective of reducing the oxidation of vanadium slag to make the slag "dry", thereby increasing the viscosity of the slag, reducing fluidity, reducing slag rolling during semi-steel tapping, and reducing the loss of vanadium slag.

[0003] CN104673964A discloses a method for modifying high-silicon vanadium-chromium slag in a converter, comprising the following steps: a. before extracting vanadium and chromium in the converter, the dosage of a slag adjusting agent is calculated according to the content of vanadium and chromium elements in vanadium-chromium iron water, if the sum of the weight percentages of vanadium and chromium in the iron water is greater than or equal to 1%, the dosage of the slag adjusting agent is 3.5-6.5 kg / tFe; if the sum of the weight percentages of vanadium and chromium in the iron water is greater than 0.5% and less than 1%, the dosage of the slag adjusting agent is 2.5-5.5 kg / tFe; b. 3-5 minutes after the converter starts to treat the vanadium-chromium iron water, the slag adjusting agent is added according to the dosage calculated in step a; c. after the converter treatment is completed, vanadium-chromium slag and semi-steel are obtained; the slag adjusting agent is composed of the following components in weight percentage: A12O3 15%-45%, MgO 0-45%, TiO2 0-5%, CaO0-3%, S<0.02%, H2O<2%, and the rest is FeO. However, in actual production, the vanadium and chromium contents have little effect on the slag state. Therefore, it is difficult to change the slag-making effect by adjusting the amount of slag regulator according to the vanadium and chromium contents.

[0004] CN104694700A discloses a slag-state regulator for extracting vanadium and chromium from high-silicon hot metal converters. The raw material composition of the regulator is SiO2 0-20%, MnO 5-25%, Na2O 0-5%, CaO 2-5%, S<0.02%, H2O<2%, and the balance is iron oxides. The regulator is suitable for the production of vanadium-chromium slag when the silicon content of hot metal is>0.25wt%. However, in actual production, when the silicon content of hot metal is>0.2%, the vanadium slag will be very thin, and this method cannot achieve the adjustment of vanadium slag for hot metal with a silicon content of ≤0.25wt%. Summary of the invention

[0005] The purpose of the present invention is to provide a method for modifying vanadium slag before vanadium extraction and steel tapping in a converter, which can effectively reduce the oxidizability of the slag, increase the viscosity of the slag, reduce the fluidity, reduce the slag rolling during semi-steel steel tapping, and reduce the loss of vanadium slag.

[0006] The present invention provides a method for modifying vanadium slag before vanadium extraction and steel tapping in a molten iron converter, which comprises the following steps:

[0007] After the oxygen blowing of the vanadium-extracting converter is completed, different amounts of slag-adjusting agents are added according to the silicon content in the molten iron; when the silicon content in the molten iron is less than 0.18wt%, no slag-adjusting agent is added; when the silicon content in the molten iron is 0.18-0.21wt%, 1.5-2.5 kg / ton of semi-steel slag-adjusting agent is added; when the silicon content in the molten iron is greater than 0.21wt%, 2.5-3.5 kg / ton of semi-steel slag-adjusting agent is added;

[0008] The slag conditioning agent is composed of a carbonaceous material, an aluminum-containing slag-forming material and a binder, wherein the carbonaceous material accounts for 80% of the total mass, the aluminum-containing slag-forming material accounts for 12-17% of the total mass, and the binder accounts for 3-8% of the total mass; the slag conditioning agent contains the following components in percentage by mass: C 65-80%, metal Al≥3%, CaO≤3%, H2O≤2%, S≤0.40%, P<0.20%, and organic matter (organic matter is tar and other substances) 5-10%.

[0009] Wherein, in the above method for modifying vanadium slag before vanadium extraction and steelmaking in molten iron converter, the particle size of the slag regulating agent is 30 to 50 mm.

[0010] Wherein, in the above method for modifying vanadium slag before vanadium extraction and steelmaking in molten iron converter, the carbonaceous material is at least one of graphite carbon, coke powder, anthracite or petroleum coke, and its fixed carbon content is ≥85%.

[0011] Wherein, in the above-mentioned method for modifying vanadium slag before vanadium extraction and steelmaking in molten iron converter, the content of metallic aluminum in the aluminum-containing slag-making material is ≥30wt%, and the rest is Al2O3.

[0012] Wherein, in the above method for modifying vanadium slag before vanadium extraction and steelmaking in molten iron converter, the binder is asphalt or starch.

[0013] Preferably, in the above method for modifying vanadium slag before vanadium extraction and steelmaking in a molten iron converter, the binder is asphalt.

[0014] Beneficial effects of the present invention:

[0015] The present invention provides an effective method for modifying vanadium slag before vanadium extraction and steelmaking in a converter. By adding a special slag conditioning agent and controlling the amount of the slag conditioning agent added in a more targeted manner according to the silicon content of molten iron, the oxidizability of the vanadium slag is successfully reduced, the slag viscosity is increased, the fluidity is reduced, the slag rolling during semi-steel steelmaking is reduced, and the loss of vanadium slag is reduced, thereby having significant economic and social benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is the SiO2-FeO phase diagram.

[0017] Figure 2 This is the phase diagram of FeO-V2O3 system. DETAILED DESCRIPTION

[0018] According to the SiO2-FeO system and FeO-V2O3 phase diagram, the inventors observed the effect of the change of FeO content in the system on the phase region. In the high FeO content area, there is a large amount of liquid phase in the system, which indicates that when the FeO content is high, the melting point of the slag is low and the fluidity is good. As the FeO content decreases, the liquid phase area decreases significantly and the solid phase area increases significantly, which means that the melting point of the slag increases, the viscosity increases, and the fluidity decreases.

[0019] Figure 1 Specifically, when the FeO content is high, the silicate phase formed by SiO2 and FeO, such as 2FeO·SiO2, has a lower melting point (1177°C), which helps maintain the fluidity of the slag. However, when the FeO content decreases, these low-melting silicate phases decrease, and more SiO2 may exist in the solid phase, causing the melting point of the slag to increase to 1205°C or even higher. This change makes the slag easier to solidify at a lower temperature, increases the cohesiveness of the slag, and reduces the loss during the steelmaking process.

[0020] Figure 2 Specifically, when the FeO content is high, the compounds formed by V2O3 and FeO, such as FeO·V2O3, have a lower melting point. As the FeO content decreases, these low-melting point compounds decrease, resulting in more V2O3 existing in the solid phase. This change makes it easier for the slag to solidify at a lower temperature, increases the viscosity and cohesiveness of the slag, and reduces loss during the steelmaking process.

[0021] In the process of vanadium extraction in the converter, the FeO content changes, which affects the ratio of the complex with silica, thereby affecting the viscosity and melting point of the slag. Therefore, the inventors conceived of changing the physical properties of the slag by controlling the FeO content.

[0022] The present invention first designs a special slag conditioning agent, which is composed of 80% carbonaceous material, 12-17% aluminum-containing slag-forming material and 3-8% binder. The FeO content in the slag is reduced by deoxidation of the carbonaceous material and the metal aluminum material, thereby changing the ratio of the FeO to silicon dioxide composition, thereby affecting the melting point and viscosity of the slag and destroying the fluidity of the slag. Among them, the use of metal aluminum can further ensure the slag conditioning effect.

[0023] At the same time, the present invention deeply analyzes the relationship between the silicon content in the molten iron and the properties of the slag, and accurately controls the amount of slag adjusting agent added: when the silicon content of the molten iron is less than 0.18wt%, no slag adjusting agent is added; when the silicon content of the molten iron is 0.18-0.21wt%, 1.5-2.5 kg / ton of semi-steel slag adjusting agent is added; when the silicon content of the molten iron is greater than 0.21wt%, 2.5-3.5 kg / ton of semi-steel slag adjusting agent is added; thereby optimizing the physical properties of the slag, reducing the oxidizability of the slag, increasing the viscosity of the vanadium slag and reducing the fluidity, reducing the "slagging" in the semi-steel discharge process, and thus improving the vanadium recovery rate.

[0024] The present invention is further described in detail below by way of examples, but the protection scope of the present invention is not limited to the scope of the examples.

[0025] In the embodiment, the slag adjusting agent used is prepared by the following method: 80% carbonaceous material, 15% aluminum-containing slag-forming material and 5% binder are evenly mixed; wherein, the carbonaceous material is graphite carbon, and its fixed carbon content is ≥85%; the aluminum-containing slag-forming material contains 30-40% metallic aluminum, and the rest is Al2O3; the binder is asphalt; and the particle size of the slag adjusting agent is 50mm.

[0026] Example 1

[0027] A 200-ton vanadium-extracting converter in a certain factory has a semi-steel output of 210 tons. After the oxygen blowing in the vanadium-extracting converter is completed, the Si content of the molten iron is 0.20%. After adding 400 kg of the above-mentioned slag-adjusting agent, the vanadium recovery rate reaches 82.3%, the V2O5 grade of the vanadium slag reaches 18.26%, and the TFe content in the vanadium slag is 27.2%.

[0028] Example 2

[0029] A 200-ton vanadium-extracting converter in a certain factory has a semi-steel output of 215 tons. After the oxygen blowing in the vanadium-extracting converter is completed, the Si content of the molten iron is 0.25%. After adding 540 kg of the above-mentioned slag-adjusting agent, the vanadium recovery rate reaches 81.43%, the V2O5 grade of the vanadium slag reaches 17.85%, and the TFe content in the vanadium slag is 26.5%.

[0030] Example 3

[0031] A 200-ton vanadium converter in a certain factory has a semi-steel output of 208 tons. After the oxygen blowing in the vanadium converter is completed, the Si content of the molten iron is 0.30%. After adding 580 kg of the above slag conditioning agent, the vanadium recovery rate reaches 83.5%, the V2O5 grade of the vanadium slag reaches 19.02%, and the TFe content in the vanadium slag is 27.5%.

[0032] Comparative Example 1

[0033] A 200t vanadium-extracting converter in a certain factory has a semi-steel output of 210t. After the oxygen blowing in the vanadium-extracting converter was completed, the Si content in the molten iron was 0.21%. No slag-adjusting materials were added before and during the blowing process, and the slag was very thin during the blowing process and at the end. The vanadium recovery rate was only 76.3%, the V2O5 grade of the vanadium slag was only 13.02%, and the TFe content in the vanadium slag was as high as 33.5%.

[0034] Comparative Example 2

[0035] A 200-ton vanadium-extracting converter in a certain factory has a semi-steel output of 215 tons. After the oxygen blowing of the vanadium-extracting converter is completed, the Si content of the molten iron is 0.19%. After adding 560 kg of the above-mentioned slag-adjusting agent, the vanadium recovery rate reaches 82%, the V2O5 grade of the vanadium slag reaches 14.3% (adding too much slag-adjusting agent will cause the vanadium slag grade to be low), and the TFe content in the vanadium slag is 26.8%.

[0036] According to experiments, when the silicon content of molten iron is 0.18-0.21wt%, adding a slag adjusting agent of up to 2.5 kg / ton of semi-steel can achieve a good slag adjusting effect. Continuing to increase the dosage will lead to a decrease in vanadium recovery rate and vanadium slag grade, and waste resources.

[0037] Comparative Example 3

[0038] A 200-ton vanadium-extracting converter in a certain factory has a semi-steel output of 210 tons. After the oxygen blowing in the vanadium-extracting converter is completed, the Si content of the molten iron is 0.23%. After adding 420 kg of the above-mentioned slag-adjusting agent, the vanadium recovery rate reaches 77%, the V2O5 grade of the vanadium slag reaches 14.2%, and the TFe content in the vanadium slag is 32%.

[0039] According to experiments, when the silicon content of molten iron is greater than 0.21wt%, if the amount of slag adjustment added is insufficient, the slag adjustment effect is poor and the recovery rate of vanadium resources is improved to a certain extent, but it is very limited.

[0040] From the above, it can be seen that the present invention significantly reduces the oxidizability of vanadium slag, increases slag viscosity, reduces fluidity, reduces slag rolling during semi-steel tapping, reduces vanadium slag loss, improves vanadium recovery rate and vanadium extraction efficiency by adding a special slag conditioning agent and strictly controlling the slag conditioning agent addition index, and has significant economic and social benefits.

Claims

1. A method for modifying vanadium slag before tapping vanadium from a molten iron converter, characterized in that: The following steps are involved: After the oxygen blowing of the vanadium-extracting converter is completed, different amounts of slag-adjusting agents are added according to the silicon content in the molten iron; when the silicon content in the molten iron is less than 0.18wt%, no slag-adjusting agent is added; when the silicon content in the molten iron is 0.18-0.21wt%, 1.5-2.5 kg / ton of semi-steel slag-adjusting agent is added; when the silicon content in the molten iron is greater than 0.21wt%, 2.5-3 kg / ton of semi-steel slag-adjusting agent is added; The slag conditioning agent is composed of a carbonaceous material, an aluminum-containing slag-forming material and a binder, wherein the carbonaceous material accounts for 80% of the total mass, the aluminum-containing slag-forming material accounts for 12-17% of the total mass, and the binder accounts for 3-8% of the total mass; the slag conditioning agent contains the following components in percentage by mass: C 65-80%, metal Al≥3%, CaO≤3%, H2O≤2%, S≤0.40%, P<0.20%, and organic matter 5-10%.

2. The method for modifying vanadium slag before vanadium extraction from molten iron converter according to claim 1, characterized in that: The particle size of the slag adjusting agent is 30 to 50 mm.

3. The method for modifying vanadium slag before vanadium extraction from molten iron converter according to claim 1, characterized in that: The carbonaceous material is at least one of graphite carbon, coke powder, anthracite or petroleum coke, and the fixed carbon content thereof is ≥85%.

4. The method for modifying vanadium slag before vanadium extraction from molten iron converter according to claim 1, characterized in that: The aluminum-containing slag-forming material has a metal aluminum content of ≥30wt%, and the rest is Al2O3.

5. The method for modifying vanadium slag before vanadium extraction from molten iron converter according to any one of claims 1 to 4, characterized in that: The binder is asphalt or starch.

6. The method for modifying vanadium slag before vanadium extraction from molten iron converter according to claim 5, characterized in that: The binder is asphalt.

Citation Information

Patent Citations

  • Modification method for high-silicon-chromium-vanadium slag of converter

    CN104673964A

  • Slag state regulator for extracting vanadium and chromium from high-silicon molten iron through converter and preparation method thereof

    CN104694700A

  • Method for recovering vanadium pentoxide from molten iron containing vanadium

    CN101648728A

  • A converter steelmaking final slag modifier and its application method

    CN102296141A

  • Method using vanadium-titanium molten iron for smelting low oxygen low carbon IF (interstitial-free) steel

    CN104060045A