Aluminum alloy strip for power battery connecting piece and preparation method of aluminum alloy strip

Through casting, cold rolling, cleaning, and coating processes, aluminum alloy strips that meet the requirements of power battery connectors are produced, solving the problem of insufficient performance in existing technologies and achieving improvements in high conductivity, corrosion resistance, and surface quality.

CN119040703APending Publication Date: 2024-11-29YONGJIE NEW MATERIAL CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411153214.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The performance of existing aluminum alloy strips cannot meet the requirements of power battery connecting pieces, especially in terms of fatigue resistance, corrosion resistance and surface quality.

Method used

Cast-rolled billets are prepared using a casting-rolling method, followed by cold rolling, cleaning, annealing, slitting, and coating treatments. The proportions of elemental components and process parameters are controlled to ensure the mechanical properties and surface quality of the aluminum alloy strip.

Benefits of technology

The prepared aluminum alloy strip has excellent tensile strength, elongation, Vickers hardness and corrosion resistance, which meets the requirements of high conductivity and aesthetics of power battery connecting pieces and can adapt to complex vibration and deformation conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040703A_ABST
    Figure CN119040703A_ABST
Patent Text Reader

Abstract

The invention discloses an aluminum alloy strip for a power battery connecting piece and a preparation method of the aluminum alloy strip, and the preparation method comprises the following steps: step S1, preparing a cast-rolling blank by adopting a cast-rolling method according to a raw material formula; s2, the cast-rolled blank is subjected to cold rolling, cleaning and annealing in sequence, and a cold-rolled strip with the thickness ranging from 1.0 mm to 2.0 mm is obtained; wherein the cleaning is carried out by adopting a hydrocarbon cleaning agent; and S3, the cold-rolled strip is sequentially subjected to slitting and film coating treatment, and the aluminum alloy strip for the power battery connecting piece is obtained. Wherein the edge burr height of the slit aluminum alloy strip for the power battery connecting piece is smaller than 0.1 mm, and the film covering is that the upper surface and the lower surface of the aluminum alloy strip for the power battery connecting piece are covered with PE films respectively. The aluminum alloy strip for the power battery connecting piece prepared by the preparation method completely meets the requirements of the power battery connecting piece.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the technical field of aluminum processing, and in particular to an aluminum alloy strip for a power battery connecting piece and a preparation method thereof. [Background technology]

[0002] The connecting plates of power batteries are mostly made of multiple layers of materials. One layer of material is a connecting layer to ensure the welding performance between the connecting plate and the pole, and the purpose of stacking multiple layers of materials is to ensure the conductivity of the connecting plate.

[0003] The base material of the connecting plate of the power battery is formed by stacking multiple layers of aluminum alloy strips and then processing them. It is generally square, trapezoidal, triangular and step-shaped. It can form a flexible area, that is, a battery soft connection, which can be used to compensate for the displacement caused by the expansion of the power battery cell to reduce the impact on the low-strength interface.

[0004] The battery soft connection can be made into a soft conductive device. The soft part uses the elasticity of the soft connection expansion joint to play a protective role. It is not restricted in the assembly angle. The hard connection is the same as the soft connection, but it does not have the above advantages of the soft connection. The battery soft connection has strong conductivity, good resistance value and electrical performance, easy to use and install, can improve conductivity, adjust equipment installation errors, and play a shock-absorbing work compensation role, which is convenient for testing and equipment maintenance. Therefore, the current connecting pieces all use soft connections.

[0005] Power batteries are mainly used in new energy vehicles. As we all know, during the driving process of the vehicle, each component will have different degrees of vibration and deformation. As an important component of new energy vehicles, the power battery needs to have a certain rigidity and flexibility to meet the vibration and deformation of the bottom of the vehicle when the vehicle moves. The connecting piece is a conductive piece between the battery cells and is a device for transmitting current. Due to the deformation of the battery pack, the connecting piece will also bend, which will have strict requirements on the fatigue resistance of the connecting piece. In order to improve the fatigue resistance of the connecting piece, it is necessary to nickel-plate the surface of the aluminum alloy strip to increase the fatigue resistance of the connecting piece through the characteristics of nickel.

[0006] In addition, the connecting piece is exposed to the outside as a transmission circuit structure, and needs to have a certain degree of corrosion resistance to avoid corrosion after long-term use, and also needs to have good surface quality for the sake of aesthetics.

[0007] In summary, the aluminum alloy strip used as a power battery connecting plate needs to have excellent mechanical properties and surface quality, as well as corrosion resistance and high electrical conductivity. However, the performance of the aluminum alloy strip in the related art cannot meet the requirements as a power battery connecting plate. [Summary of the invention]

[0008] The purpose of the embodiments of the present invention is to provide an aluminum alloy strip for a power battery connecting piece and a preparation method thereof, so as to solve the problem that the performance of the aluminum alloy strip in the related art cannot meet the requirements of being a power battery connecting piece.

[0009] In a first aspect, an embodiment of the present invention provides a method for preparing an aluminum alloy strip for a power battery connecting sheet, comprising the following steps:

[0010] Step S1, preparing a cast-rolled billet by a casting-rolling method according to the following raw material formula;

[0011] The components and mass percentages of the raw material formula are: Si=0.07-0.08%, Fe=0.17-0.30%, Cu=0.06-0.22%, Mg<0.01%, Ti=0.01-0.03%, Al≥99.60%, wherein the mass fraction ratio of element Fe to element Si is 2.3-2.4;

[0012] Step S2, cold rolling, cleaning and annealing the cast-rolled billet in sequence to obtain a cold-rolled strip with a thickness of 1.0 to 2.0 mm; wherein the cleaning is performed using a hydrocarbon cleaning agent, and the annealing is performed after the temperature of the cast-rolled billet reaches 290±5° C. and is kept warm for 2 to 4 hours;

[0013] Step S3, slitting and laminating the cold-rolled strip in sequence to obtain an aluminum alloy strip for a power battery connecting piece; wherein the burr height of the edge of the aluminum alloy strip for a power battery connecting piece after the slitting process is less than 0.1 mm, and the laminating process is to coat the upper surface and the lower surface of the aluminum alloy strip for a power battery connecting piece with a PE film respectively.

[0014] Preferably, in step S1, the steps of the casting and rolling method include in sequence: batching, smelting, stirring, first refining, first standing, first slag removal, adding metal additives, second standing, second slag removal, furnace pouring, second refining, third slag removal, third standing, degassing, filtering and casting and rolling; wherein, the smelting is carried out in a smelting furnace, and the stirring, first refining, first standing, first slag removal, second standing and second slag removal are all carried out in the smelting furnace, and the furnace pouring is to pour the molten aluminum in the smelting furnace into a holding furnace, and the second refining, third slag removal and third standing are all carried out in the holding furnace.

[0015] Preferably, in the step S1, the stirring is performed continuously in multiple batches and once every 2 to 3 hours; and the second refining is performed continuously in multiple batches and once every 4 hours.

[0016] Preferably, in step S1, the stirring is performed by a forklift; the filtering is performed by a filter box, the furnace gas temperature of the filter box is 750-760°C during filtering, and the liquid level of the front box is increased by 2-3cm relative to 24cm; the casting and rolling is performed by an inclined rolling mill, and the rolling speed during casting and rolling is 1100±50mm / min.

[0017] Preferably, in the step S1, the casting is performed in an environment where the air humidity is less than or equal to 80% and the air dew point temperature is greater than or equal to 8°C.

[0018] Preferably, in step S2, the hydrocarbon cleaning agent includes isomeric hydrocarbons, normal hydrocarbons and cycloalkanes, and the mass ratio of the isomeric hydrocarbons, the normal hydrocarbons and the cycloalkanes is 7:2:1.

[0019] Preferably, in step S2, the cold rolling is performed by a cold rolling mill, and the rotation directions of the rollers and the grinding wheel in the cold rolling mill are opposite.

[0020] Preferably, in step S3, the slitting process is performed by a slitting machine, and then a film laminating roller is respectively provided above and below the rear of the slitting machine, so that the two film laminating rollers are respectively located on the upper and lower surfaces of the aluminum alloy strip for the power battery connecting sheet after slitting, the material of the film laminating roller is polyurethane, the roller surface hardness of the film laminating roller is 80-85HSA, the roughness of the film laminating roller is Ra0.6-0.8μm, and the film laminating pressure of the film laminating roller is 0.15-0.2Mpa.

[0021] In a second aspect, an embodiment of the present invention provides an aluminum alloy strip for a power battery connecting piece, which is made by the above-mentioned method for preparing the aluminum alloy strip for a power battery connecting piece, and the aluminum alloy strip for a power battery connecting piece is applied to the power battery connecting piece of a new energy vehicle.

[0022] Compared with the related art, the preparation method of the aluminum alloy strip for the power battery connecting piece in the present invention comprises the following steps: preparing a cast-rolled billet by a casting-rolling method according to a raw material formula; cold rolling, cleaning and annealing the cast-rolled billet in sequence to obtain a cold-rolled strip with a thickness of 1.0 to 2.0 mm; slitting and laminating the cold-rolled strip in sequence to obtain an aluminum alloy strip for the power battery connecting piece with a thickness of 1.0 to 2.0 mm, and a tensile strength of 105 to 145 MPa, a tensile strength of 165 to 185 MPa in the nickel-plated area, an elongation greater than 4%, and a Vickers hardness value of HV 34~42, bending angle is 135°, bending back and forth for many times without cracking, that is, excellent mechanical properties, no color difference and bright line on the surface, that is, excellent surface quality, salt spray test rating and judgment according to national standard GB / T6461-2002, after continuous corrosion for 96h, the black corrosion rate is 0.1~0.15%, the judgment level is higher than level 8, that is, excellent corrosion resistance, conductivity is greater than 3.5*10 7 S / m, fully meets the requirements as a power battery connector.

Brief Description of the Drawings

[0023] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative work, among which:

[0024] Figure 1 A schematic flow chart of the steps of a method for preparing an aluminum alloy strip for a power battery connecting piece provided in an embodiment of the present invention. [Specific implementation method]

[0025] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] The embodiment of the present invention provides a method for preparing an aluminum alloy strip for a power battery connecting sheet, Figure 1 As shown, it includes the following steps:

[0027] Step S1, preparing a cast-rolled billet by a casting-rolling method according to a raw material formula.

[0028] The components and mass percentages of the raw material formula are as follows: Si=0.07-0.08%, Fe=0.17-0.30%, Cu=0.06-0.22%, Mg<0.01%, Ti=0.01-0.03%, Al≥99.60%, and the mass fraction ratio of element Fe to element Si is 2.3-2.4.

[0029] The elements Fe, Cu and Ti are prepared as alloy elements according to the above mass percentages and added as metal additives; the remaining elements are not added separately, and the element Al can be prepared by remelting aluminum ingots with a mass percentage of 99.80-99.85% to strictly control the content of impurity elements.

[0030] By controlling the mass fraction ratio of element Fe and element Si, it is easy to form α phase Fe 2 SiAl 8 , which can avoid a large amount of hard and brittle phase β phase FeSiAl 3 The formation of β phase will lead to a sharp deterioration of organizational properties; element Cu can generate strengthening phase CuAl 2 , to refine the grains and improve the strength of the aluminum alloy strip, and the electrode potential of the element Cu is higher than that of Al. The Cu compounds on the surface of the aluminum alloy strip and around the grain boundary can serve as the starting point of corrosion to improve the bonding strength of the nickel-plated area, so as to adapt to the complex working conditions of the joint of the power battery connecting piece where continuous vibration and deformation occur. Therefore, the obtained aluminum alloy strip has excellent organization, which is convenient for improving its stamping performance.

[0031] The steps of the casting and rolling method include: batching, smelting, stirring, first refining, first standing, first slag removal, adding metal additives, second standing, second slag removal, furnace pouring, second refining, third slag removal, third standing, degassing, filtering and casting and rolling; wherein, the smelting is carried out in a smelting furnace, and the stirring, first refining, first standing, first slag removal, second standing and second slag removal are all carried out in the smelting furnace, and the furnace pouring is to pour the molten aluminum in the smelting furnace into a holding furnace, and the second refining, third slag removal and third standing are all carried out in the holding furnace.

[0032] The stirring is carried out in batches without interruption and once every 2 to 3 hours, so that each element can be uniform. In particular, the density of element Cu is greater than that of Al, so stirring can avoid the inhomogeneity caused by the macro segregation of element Cu.

[0033] The second refining is carried out in multiple batches without interruption and is refined every 4 hours.

[0034] The stirring is carried out by a forklift; the filtering is carried out by a filter box, and the furnace gas temperature of the filter box is 750-760°C during filtering to avoid rapid grain growth caused by excessive temperature; the casting and rolling is carried out by an inclined rolling mill, and the rolling speed during casting and rolling is 1100±50mm / min, which can accelerate the cooling and recrystallization of the aluminum water to 200-220°C to avoid grain growth; the liquid level height of the front box is increased by 2-3cm relative to 24cm, which can increase the static pressure of the aluminum water during crystallization to refine the grains.

[0035] The casting and rolling is carried out in an environment where the air humidity is less than or equal to 80% and the air dew point temperature is greater than or equal to 8°C, because when the air humidity is greater than 80% and the air dew point temperature is less than 8°C, the probability of producing coarse grains is 60-65%, which will affect the cooling of the rolls of the inclined rolling mill, and then cause uneven cooling of the plate surface of the cast-rolled billet, resulting in coarse grains on the local or entire plate surface. The control of air humidity and air dew point temperature is that the production workshop closes doors and windows and uses a dehumidifier to reduce the air humidity and increase the air dew point temperature, which can significantly improve the problem of coarse grains.

[0036] Step S2, cold rolling, cleaning and annealing the cast-rolled billet in sequence to obtain a cold-rolled strip with a thickness of 1.0 to 2.0 mm.

[0037] Among them, the required tin plating thickness of the aluminum alloy strip is generally 5 to 15 μm. The compressive yield strength of the aluminum alloy strip after nickel plating will increase by about 10 MPa, but the surface cleanliness of the aluminum alloy strip needs to be less than or equal to 80 RFU to ensure the surface quality of the power battery connector after tin plating. If the RFU is larger, it means that the content of residual pollutants on the surface of the aluminum alloy strip is higher, and the corresponding surface quality of the power battery connector after tin will be worse; among them, RFU is the data of relative fluorescence unit, which indicates the surface cleanliness of the aluminum alloy strip.

[0038] The cleaning is performed using a hydrocarbon cleaning agent, which can remove aluminum powder, iron powder, oil stains, dust and other foreign matter on the surface of the aluminum alloy strip to ensure the surface quality of the aluminum alloy strip. The hydrocarbon cleaning agent is a non-polar organic solvent with good dissolving power, low surface tension and better wetting performance. According to the principle of "like dissolves like", it is a non-polar petroleum fraction like most lubricating oils, rust-proof oils and machining oils. Therefore, the effect of the hydrocarbon cleaning agent in cleaning these mineral oils is better than that of traditional halogenated hydrocarbons and water-based cleaning agents.

[0039] The hydrocarbon cleaning agent includes isomeric hydrocarbons, normal hydrocarbons and cycloalkanes, and the mass ratio of the isomeric hydrocarbons, the normal hydrocarbons and the cycloalkanes is 7:2:1. Among them, isomeric hydrocarbons are one of the main components of the hydrocarbon cleaning agent, have good solubility and low surface tension, and can effectively clean various oil stains and impurities; normal hydrocarbons play a role in increasing the stability and solubility of the cleaning agent in the hydrocarbon cleaning agent, but their volatility is low, which may affect the drying speed of the cleaning agent, and cycloalkanes play a role in adjusting the solubility and volatility of the cleaning agent in the hydrocarbon cleaning agent, and can also increase the anti-rust performance of the cleaning agent, which can effectively protect the aluminum alloy strip from corrosion after cleaning.

[0040] The cold rolling is performed by a cold rolling mill, and the rollers in the cold rolling mill adopt a reverse grinding process and rotate clockwise and counterclockwise opposite to the grinding wheel. Compared with the traditional same-direction grinding process, the reverse grinding process will reduce the cutting thickness of the abrasive grains on the cutting surface of the grinding wheel and the roller, and the load of a single abrasive grain will be reduced, which will eventually reduce the relative feed amount of the grinding wheel and reduce the roughness, so that a roller surface with a uniform and delicate surface can be obtained. Accordingly, the surface quality of the cold-rolled strip obtained by cold rolling is excellent.

[0041] The annealing is carried out after the temperature of the cast and rolled billet reaches 290±5° C. and the billet is kept at this temperature for 2 to 4 hours.

[0042] Step S3, sequentially slitting and laminating the cold-rolled strip to obtain an aluminum alloy strip for a power battery connecting piece.

[0043] Among them, the burr height of the edge of the aluminum alloy strip for power battery connecting piece after the slitting process is less than 0.1 mm, and the coating process is to coat the upper surface and the lower surface of the aluminum alloy strip for power battery connecting piece with PE film respectively.

[0044] The slitting process is carried out by a slitting machine, and a film-laminating roller is arranged at the upper and lower positions of the rear position of the slitting machine, so that the two film-laminating rollers are respectively located on the upper and lower surfaces of the aluminum alloy strip for the power battery connector after slitting. The film-laminating roller is made of polyurethane, the roller surface hardness of the film-laminating roller is Shore hardness 80-85HSA, the roughness of the film-laminating roller is Ra0.6-0.8μm, and the film-laminating pressure of the film-laminating roller is 0.15-0.2Mpa. Among them, the film-laminating roller is used to apply PE film on the upper and lower surfaces of the aluminum alloy strip for the power battery connector.

[0045] Compared with traditional nitrile rubber laminating rollers, polyurethane laminating rollers are more resistant to water, alkali and temperature, and are suitable for working at temperatures of -20 to 100°C; the surface hardness of the laminating roller is uniform, and there are no bubbles, impurities or mechanical damage on the surface to avoid abnormal degumming.

[0046] After the upper and lower surfaces of the aluminum alloy strip for the power battery connecting plate are respectively covered with PE films, no film peeling occurs on the surface of the aluminum alloy strip. The reason for the peeling is that the PE film and the aluminum powder or aluminum chips accumulated on the surface of the aluminum alloy strip in the rolling texture produce stress concentration. After the film is peeled, the aluminum powder or aluminum chips adhere to the PE film, resulting in poor peeling on the surface of the strip.

[0047] The aluminum alloy strip prepared by the preparation method of the aluminum alloy strip for the power battery connector is subjected to a salt spray corrosion test. When the salt spray particles settle and adhere to the surface of the material, they quickly absorb moisture and dissolve into a chloride aqueous solution. This chloride aqueous solution or the dissociated chloride ions penetrate into the material system through the micropores on the surface of the material, thereby causing aging of the material or corrosion of the metal. After 96 hours of continuous corrosion, the black corrosion rate is 0.1-0.15%. According to the national standard GB / T 6461-2002, the salt spray test rating and judgment are higher than level 8. The excellent internal organization can make it have excellent corrosion resistance.

[0048] Compared with the related art, the method for preparing the aluminum alloy strip for the power battery connecting piece in the present embodiment comprises the following steps: preparing a cast-rolled billet by a casting-rolling method according to a raw material formula; cold rolling, cleaning and annealing the cast-rolled billet in turn to obtain a cold-rolled strip with a thickness of 1.0 to 2.0 mm; slitting and laminating the cold-rolled strip in turn to obtain an aluminum alloy strip for the power battery connecting piece with a thickness of 1.0 to 2.0 mm, and a tensile strength of 105 to 145 MPa, a tensile strength of 165 to 185 MPa in the nickel-plated area, an elongation greater than 4%, and a Vickers hardness value of HV 34~42, bending angle is 135°, bending back and forth for many times without cracking, that is, excellent mechanical properties, no color difference and bright line on the surface, that is, excellent surface quality, salt spray test rating and judgment according to national standard GB / T6461-2002, after continuous corrosion for 96h, the black corrosion rate is 0.1~0.15%, the judgment level is higher than level 8, that is, excellent corrosion resistance, conductivity is greater than 3.5*10 7 S / m, fully meets the requirements as a power battery connector.

[0049] The present invention also provides another embodiment, an aluminum alloy strip for a power battery connecting sheet, which is made by the preparation method of the aluminum alloy strip for a power battery connecting sheet in the above embodiment, and the aluminum alloy strip for a power battery connecting sheet is applied to the power battery connecting sheet of a new energy vehicle.

[0050] Since the aluminum alloy strip for power battery connecting tabs in the present embodiment is made by the preparation method of the aluminum alloy strip for power battery connecting tabs in the above embodiment, the aluminum alloy strip for power battery connecting tabs in the present embodiment can also achieve the technical effect achieved by the preparation method of the aluminum alloy strip for power battery connecting tabs in the above embodiment, which will not be elaborated here.

[0051] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A method for preparing an aluminum alloy strip for a power battery connecting piece, characterized in that: The method for preparing the aluminum alloy strip for the power battery connecting sheet comprises the following steps: Step S1, preparing a cast-rolled billet by a casting-rolling method according to the following raw material formula; The components and mass percentages of the raw material formula are: Si=0.07-0.08%, Fe=0.17-0.30%, Cu=0.06-0.22%, Mg<0.01%, Ti=0.01-0.03%, Al≥99.60%, wherein the mass fraction ratio of element Fe to element Si is 2.3-2.4; Step S2, cold rolling, cleaning and annealing the cast-rolled billet in sequence to obtain a cold-rolled strip with a thickness of 1.0 to 2.0 mm; wherein the cleaning is performed using a hydrocarbon cleaning agent, and the annealing is performed after the temperature of the cast-rolled billet reaches 290±5° C. and is kept warm for 2 to 4 hours; Step S3, slitting and laminating the cold-rolled strip in sequence to obtain an aluminum alloy strip for a power battery connecting piece; wherein the burr height of the edge of the aluminum alloy strip for a power battery connecting piece after the slitting process is less than 0.1 mm, and the laminating process is to coat the upper surface and the lower surface of the aluminum alloy strip for a power battery connecting piece with a PE film respectively.

2. The method for preparing the aluminum alloy strip for power battery connecting sheet according to claim 1, characterized in that: In step S1, the steps of the casting and rolling method include in sequence: batching, smelting, stirring, first refining, first standing, first slag removal, adding metal additives, second standing, second slag removal, furnace pouring, second refining, third slag removal, third standing, degassing, filtering and casting and rolling; wherein, the smelting is carried out in a smelting furnace, and the stirring, first refining, first standing, first slag removal, second standing and second slag removal are all carried out in the smelting furnace, and the furnace pouring is to pour the molten aluminum in the smelting furnace into a holding furnace, and the second refining, third slag removal and third standing are all carried out in the holding furnace.

3. The method for preparing the aluminum alloy strip for power battery connecting sheet according to claim 2, characterized in that: In the step S1, the stirring is performed continuously in multiple batches and once every 2 to 3 hours; the second refining is performed continuously in multiple batches and once every 4 hours.

4. The method for preparing the aluminum alloy strip for power battery connecting sheet according to claim 2, characterized in that: In the step S1, the stirring is performed by a forklift; the filtering is performed by a filter box, and the furnace gas temperature of the filter box is 750-760°C during filtering; the casting and rolling is performed by an inclined rolling mill, and the rolling speed during casting and rolling is 1100±50mm / min, and the liquid level of the front box is increased by 2-3cm relative to 24cm.

5. The method for preparing the aluminum alloy strip for power battery connecting sheet according to claim 2, characterized in that: In the step S1, the casting is performed in an environment where the air humidity is less than or equal to 80% and the air dew point temperature is greater than or equal to 8°C.

6. The method for preparing the aluminum alloy strip for power battery connecting sheet according to claim 1, characterized in that: In the step S2, the hydrocarbon cleaning agent includes isomeric hydrocarbons, normal hydrocarbons and cycloalkanes, and the mass ratio of the isomeric hydrocarbons, the normal hydrocarbons and the cycloalkanes is 7:2:

1.

7. The method for preparing the aluminum alloy strip for power battery connecting sheet according to claim 1, characterized in that: In the step S2, the cold rolling is performed by a cold rolling mill, and the rotation directions of the rollers and the grinding wheel in the cold rolling mill are opposite.

8. The method for preparing the aluminum alloy strip for power battery connecting sheet according to claim 1, characterized in that: In the step S3, the slitting process is performed by a slitting machine, and a film laminating roller is arranged above and below the rear position of the slitting machine, so that the two film laminating rollers are respectively located on the upper and lower surfaces of the aluminum alloy strip for the power battery connecting piece after slitting. The material of the film laminating roller is polyurethane, the roller surface hardness of the film laminating roller is 80-85HSA, the roughness of the film laminating roller is Ra0.6-0.8μm, and the film laminating pressure of the film laminating roller is 0.15-0.2Mpa.

9. An aluminum alloy strip for a power battery connector, characterized in that: The aluminum alloy strip for power battery connecting piece is made by the preparation method of the aluminum alloy strip for power battery connecting piece according to any one of claims 1 to 8, and the aluminum alloy strip for power battery connecting piece is applied to power battery connecting pieces of new energy vehicles.