In-mold inoculation block for preparing thick and large-section ductile iron casting and preparation process of in-mold inoculation block
Through the use of high-aluminum content in-form incubation blocks, problems such as graphite floating in the production of thick and large-section ductile iron parts are solved, the strength and hardness of the castings are improved, and more efficient casting production is achieved.
Patent Information
- Application Number
- CN202411175028.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-29
AI Technical Summary
When producing thick and large-section ductile iron parts, the cooling speed of the castings is slow and solidified for a long time, and defects such as graphite floating, fragmented graphite, spheroidization decline and anti-white opening are prone to occur, which affects the strength of the final casting.
Using high alumina content intra-type incubation blocks, the specific ratio and process of ferrosilicon, calcium silicon and aluminum ingots for remelting can promote graphitization, improve graphite morphology and distribution, increase the number of eutectic groups, and refine matrix structure. , improve the strength of the castings.
Through the use of high-aluminum content incubation blocks, the tendency of white mouth is reduced, the tensile strength, yield strength and hardness of the casting are improved, and the internal comprehensive performance of the casting is improved.
Smart Images

Figure BDA0005010491410000071
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of metal materials, and in particular to an in-mold inoculant block for preparing thick and large-section ductile iron castings and a preparation process thereof. Background Art
[0002] In recent years, with the advancement of ductile iron casting production technology and the emergence of new application fields, the production of thick and large-section ductile iron castings has seen a booming development. For example, with the rapid development of wind power generation, the hubs, bases and other thick and large-section castings in wind power generation equipment are all produced with ductile iron; with the resurgence of the shipbuilding industry worldwide, the engine cylinders and cylinder heads of large ship diesel engines are also increasingly produced with ductile iron castings. When producing thick and large-section ductile iron castings, due to the slow cooling speed and long solidification time of the castings, many defects such as graphite floating, fragmented graphite, spheroidization recession and white mouth are prone to occur during the production process of the castings, thus affecting the strength of the final castings. Summary of the invention
[0003] In order to improve the strength of the final casting, the present application provides an in-mold inoculant block for preparing thick and large-section ductile iron castings and a preparation process thereof.
[0004] In the first aspect, the present application provides an in-mold inoculant for preparing thick and large-section ductile iron castings, which adopts the following technical solution: The invention discloses an in-mold inoculant for preparing thick and large-section ductile iron castings. The inoculant comprises the following components in weight percentage: 70-80% silicon, 0.5-1.5% calcium, 3.2-4.5% aluminum, and the balance iron.
[0005] By adopting the above technical scheme, in the production process of castings, the inoculant block in the present application is added. The inoculant block in the present application has a high aluminum content, which can promote graphitization, reduce the tendency of white cast iron, improve the morphology and distribution of graphite, increase the number of eutectic clusters, and refine the matrix structure, thereby improving the strength of the final casting.
[0006] In a specific possible implementation mode, the raw materials of the inoculant include: ferrosilicon, calcium silicon, and aluminum ingots for remelting.
[0007] In a specific implementation manner, the weight ratio of the ferrosilicon, the calcium silicon, and the aluminum ingot for remelting is 100:(2-3):(4-5).
[0008] By adopting the above technical scheme, using ferrosilicon, calcium silicon and aluminum ingots for remelting as raw materials, and further limiting the ratio of ferrosilicon, calcium silicon and aluminum ingots for remelting, an in-mold inoculant with a high aluminum content can be produced.
[0009] In a specific embodiment, the inoculum is in the shape of a rectangular cone.
[0010] By adopting the above technical solution, the rectangular trapezoidal setting increases the surface area of the inoculant. The inoculant with a large surface area has a large contact area with the molten metal, and the heat transfer and solute diffusion rates are fast, so that the inoculant is evenly dissolved. The melting process of the inoculant is carried out synchronously with the casting process, thereby improving the inherent comprehensive performance of the casting.
[0011] In the second aspect, the present application provides a process for preparing an in-mold inoculant block for preparing thick and large-section ductile iron castings, which adopts the following technical solution: A process for preparing an in-mold inoculant block for preparing thick and large-section ductile iron castings comprises the following steps: Ingredients: crush ferrosilicon, calcium silicon and aluminum ingots for remelting respectively and set aside; Charging: First add ferrosilicon and calcium silicon into the electric furnace, and then add aluminum ingots for remelting into the electric furnace; Melting: After the charge is put into the furnace, the power can be increased for melting. The raw materials in the furnace are heated until they are melted, and then stirred to remove the scum. After confirming that there is no raw material, the furnace can be taken out to obtain the inoculant melt; Pouring: reduce the current of the electric furnace, tilt the furnace under the protection of nitrogen, pour the inoculant melt into the inoculant metal mold to obtain the inoculant rough material; Cleaning: Wait for the rough material of the inoculant to cool down completely before taking it out, and clean the gate, runner and other parts to get the finished inoculant.
[0012] By adopting the above technical scheme, the raw materials of ferrosilicon, calcium silicon and aluminum ingots for remelting are first crushed, and then ferrosilicon and calcium silicon are added into the electric furnace, and then the aluminum ingots for remelting are added, heated to melt, scum is removed, the furnace is tilted under the protection of nitrogen, poured into a casting mold for casting, and finally cleaned to obtain a finished inoculant.
[0013] In a specific possible implementation mode, in the batching step, the particle size of the ferrosilicon and the calcium silicon is 5-20 mm, and the aluminum ingot for remelting is a block of 50×50×50 mm.
[0014] By adopting the above technical solution, the crushing size of the raw materials ferrosilicon, calcium silicon and aluminum ingots for remelting is further limited, which facilitates the smelting of the raw materials.
[0015] In a specific embodiment, in the smelting step, the power is 100-200 kW, the voltage is 300-500 V, and the current is 240-450 A.
[0016] In a specific embodiment, during the pouring step, the current of the electric furnace is reduced to 0A.
[0017] By adopting the above technical solution, the specific parameters in the smelting and pouring steps are further limited, which is beneficial to the molding of the finished inoculant.
[0018] In a third aspect, the present application provides a thick and large-section ductile iron casting, which adopts the following technical solution: A thick and large-section ductile iron casting is made from the in-mold inoculated block used for preparing thick and large-section ductile iron castings.
[0019] By adopting the above technical solution, the iron parts made by using the in-mold inoculated block in the present application have strong tensile strength, yield strength and hardness.
[0020] In a specific embodiment, the cast iron part comprises the following components in weight percentage: C accounts for 3.3-3.7%; Si accounts for 2.8-3.7%; Mn≤0.3%; P≤0.05%; S≤0.02%; Cu≤0.1%; Mg accounts for 0.04-0.06%; RE accounts for 0.01-0.03%.
[0021] In summary, the present application includes at least one of the following beneficial technical effects: 1. The inoculant in this application has a high aluminum content, which can promote graphitization, reduce the tendency of white cast iron, improve the morphology and distribution of graphite, increase the number of eutectic clusters, and refine the matrix structure, thereby improving the strength of the final casting; 2. The method of the present application first crushes the raw materials of ferrosilicon, calcium silicon and aluminum ingot for remelting, then adds ferrosilicon and calcium silicon into an electric furnace, then adds aluminum ingot for remelting, heats until melted, removes scum, tilts the furnace under the protection of nitrogen, pours into a casting mold for casting, and finally cleans to obtain a finished inoculant; 3. The thick and heavy-section ductile iron castings in the present application are made from in-mold inoculated blocks used for preparing thick and heavy-section ductile iron castings, and have strong tensile strength, yield strength and hardness. DETAILED DESCRIPTION
[0022] The present application is further described in detail below with reference to the embodiments.
[0023] All raw materials in the examples can be obtained from the market. Among them, the ferrosilicon grade is FeSi75-A, and the chemical composition is Si, 72.0-80.0%; Al, 0%; Ca, 0; Mn<0.4%; Cr<0.3%; P<0.035%; S<0.020; C<0.10%; the balance is Fe; Calcium silicon grade: Ca28Si60, chemical composition: Ca>28%; Si, 50-65%; C<1.2%; Al<2.4%; P<0.04%; S<0.06%; Aluminum ingot for remelting: Al99.60b, chemical composition: Al>99.60; Si<0.16%; Fe<0.25; Cu<0.01; Ga<0.03; Mg<0.03; Zn<0.03; Chemical composition of Q10 pig iron: C>3.3%; Si≤0.1%; Mn, 0.2-0.5%; S, 0.02-0.04%; P, 0.05-0.07%. Example
[0024] Example 1 Embodiment 1 provides a process for preparing an in-mold inoculant for preparing thick and large-section ductile iron castings, comprising the following steps: batching: crushing ferrosilicon, calcium silicon, and aluminum ingots for remelting respectively, so that the particle size of ferrosilicon and calcium silicon is 5-20 mm, and the aluminum ingots for remelting are 50×50×50 mm blocks for standby use; wherein the weight ratio of ferrosilicon, calcium silicon, and aluminum ingots for remelting is 100:2:4; Charging: First add ferrosilicon and calcium silicon into the electric furnace, and then add aluminum ingots for remelting into the electric furnace; Melting: After the charge is put into the furnace, adjust the power of the electric furnace to 100kw, the voltage to 300V, and the current to 240A, heat the raw materials in the furnace until they are melted, then stir and skim off the scum, and after confirming that there is no raw material, take it out of the furnace to obtain the inoculant melt; Pouring: reduce the current of the electric furnace to 0A, tilt the furnace under the protection of nitrogen, pour the inoculant melt into the inoculant metal mold to obtain the inoculant rough material; Cleaning: Wait for the rough inoculant to cool completely before taking it out, remove the gate, runner and other parts, and obtain a finished inoculant in the shape of a rectangular table; the inoculant includes the following components in weight percentage: 70% silicon, 0.5% calcium, 3.2% aluminum, and the balance is iron.
[0025] Example 2 Embodiment 2 provides a process for preparing an in-mold inoculant for preparing thick and large-section ductile iron castings, comprising the following steps: batching: crushing ferrosilicon, calcium silicon, and aluminum ingots for remelting respectively, so that the particle size of ferrosilicon and calcium silicon is 5-20 mm, and the aluminum ingots for remelting are 50×50×50 mm blocks for standby use; wherein the weight ratio of ferrosilicon, calcium silicon, and aluminum ingots for remelting is 100:2.5:4.5; Charging: First add ferrosilicon and calcium silicon into the electric furnace, and then add aluminum ingots for remelting into the electric furnace; Melting: After the charge is put into the furnace, adjust the power of the electric furnace to 100kw, the voltage to 300V, and the current to 240A, heat the raw materials in the furnace until they are melted, then stir and skim off the scum, and after confirming that there is no raw material, take it out of the furnace to obtain the inoculant melt; Pouring: reduce the current of the electric furnace to 0A, tilt the furnace under the protection of nitrogen, pour the inoculant melt into the inoculant metal mold to obtain the inoculant rough material; Cleaning: Wait for the rough inoculant to cool completely before taking it out, remove the gate, runner and other parts, and obtain a finished inoculant in the shape of a rectangular table; the inoculant includes the following components in weight percentage: 75% silicon, 1% calcium, 3.8% aluminum, and the balance is iron.
[0026] Example 3 Embodiment 3 provides a process for preparing an in-mold inoculant for preparing thick and large-section ductile iron castings, comprising the following steps: batching: crushing ferrosilicon, calcium silicon, and aluminum ingots for remelting respectively, so that the particle size of ferrosilicon and calcium silicon is 5-20 mm, and the aluminum ingots for remelting are 50×50×50 mm blocks for standby use; wherein the weight ratio of ferrosilicon, calcium silicon, and aluminum ingots for remelting is 100:3:5; Charging: First add ferrosilicon and calcium silicon into the electric furnace, and then add aluminum ingots for remelting into the electric furnace; Melting: After the charge is put into the furnace, adjust the power of the electric furnace to 100kw, the voltage to 300V, and the current to 240A, heat the raw materials in the furnace until they are melted, then stir and skim off the scum, and after confirming that there is no raw material, take it out of the furnace to obtain the inoculant melt; Pouring: reduce the current of the electric furnace to 0A, tilt the furnace under the protection of nitrogen, pour the inoculant melt into the inoculant metal mold to obtain the inoculant rough material; Cleaning: Wait for the rough inoculant to cool completely before taking it out, remove the gate, runner and other parts, and obtain a finished inoculant in the shape of a rectangular table; the inoculant includes the following components in weight percentage: 80% silicon, 1.5% calcium, 4.5% aluminum, and the balance is iron.
[0027] Example 4 Embodiment 4 provides a process for preparing an in-mold inoculant for preparing thick and large-section ductile iron castings, comprising the following steps: batching: crushing ferrosilicon, calcium silicon, and aluminum ingots for remelting respectively, so that the particle size of ferrosilicon and calcium silicon is 5-20 mm, and the aluminum ingots for remelting are 50×50×50 mm blocks for standby use; wherein the weight ratio of ferrosilicon, calcium silicon, and aluminum ingots for remelting is 100:2.5:4.5; Charging: First add ferrosilicon and calcium silicon into the electric furnace, and then add aluminum ingots for remelting into the electric furnace; Melting: After the charge is put into the furnace, adjust the power of the electric furnace to 150kw, the voltage to 400V, and the current to 340A, heat the raw materials in the furnace until they are melted, then stir and skim off the scum, and after confirming that there is no raw material, take it out of the furnace to obtain the inoculant melt; Pouring: reduce the current of the electric furnace to 0A, tilt the furnace under the protection of nitrogen, pour the inoculant melt into the inoculant metal mold to obtain the inoculant rough material; Cleaning: Wait for the rough inoculant to cool completely before taking it out, remove the gate, runner and other parts, and obtain a finished inoculant in the shape of a rectangular table; the inoculant includes the following components in weight percentage: 73% silicon, 1% calcium, 3.7% aluminum, and the balance is iron.
[0028] Example 5 Embodiment 5 provides a process for preparing an in-mold inoculant for preparing thick and large-section ductile iron castings, comprising the following steps: batching: crushing ferrosilicon, calcium silicon, and aluminum ingots for remelting respectively, so that the particle size of ferrosilicon and calcium silicon is 5-20 mm, and the aluminum ingots for remelting are 50×50×50 mm blocks for standby use; wherein the weight ratio of ferrosilicon, calcium silicon, and aluminum ingots for remelting is 100:2.5:4.5; Charging: First add ferrosilicon and calcium silicon into the electric furnace, and then add aluminum ingots for remelting into the electric furnace; Melting: After the charge is put into the furnace, adjust the power of the electric furnace to 200kw, the voltage to 500V, and the current to 450A, heat the raw materials in the furnace until they are melted, then stir and skim off the scum, and after confirming that there is no raw material, take it out of the furnace to obtain the inoculant melt; Pouring: reduce the current of the electric furnace to 0A, tilt the furnace under the protection of nitrogen, pour the inoculant melt into the inoculant metal mold to obtain the inoculant rough material; Cleaning: Wait for the rough inoculant to cool completely before taking it out, remove the gate, runner and other parts, and obtain a finished inoculant in the shape of a rectangular table; the inoculant includes the following components in weight percentage: 76% silicon, 1% calcium, 3.7% aluminum, and the balance is iron.
[0029] Comparative Example Comparative Example 1 Comparative Example 1 provides a preparation process of an inoculant, comprising the following steps: First, add scrap steel to the bottom of the acidic medium frequency furnace, cover it with ferromanganese alloy, then insert a graphite carbon rod vertically in the middle of the acidic medium frequency furnace, and then add 75% ferrosilicon broken into small pieces, and then heat the acidic medium frequency furnace to 1530°C to melt the solid matter in the furnace; after melting, use a slag collector to deslag the liquid in the furnace once, and then add aluminum wire to melt it to form molten iron; after preheating the ladle to 65°C, put silicon-calcium alloy and rare earth magnesium ferrosilicon at the bottom of the ladle, and then pour the molten iron into the ladle to melt it to form final molten iron; pour the final molten iron, and take out the inoculant 11 minutes after the pouring is completed; the weight ratio of 75% ferrosilicon, silicon-calcium alloy, rare earth magnesium ferrosilicon, aluminum wire, ferromanganese alloy and scrap steel is 75:2:5:3:5:10.
[0030] Application Examples Application Example 1 Application Example 1 provides a method for preparing a thick and large-section ductile iron casting, comprising the following steps: High-quality scrap steel, Q10 pig iron and recycled materials are sequentially added to a coreless medium frequency induction furnace for smelting. After all the raw materials are melted, the scum is scraped off, the composition of the molten iron is adjusted, and the inoculant block in Example 1 is placed in the pouring box to obtain a thick and large-section ductile iron casting.
[0031] Application Example 2 Application Example 2 provides a method for preparing a thick and large-section ductile iron casting, comprising the following steps: High-quality scrap steel, Q10 pig iron and recycled materials are added to a coreless medium-frequency induction furnace in sequence for smelting. After all the raw materials are melted, the slag is scraped off, the composition of the molten iron is adjusted, and the inoculant block in Example 2 is placed in the pouring box to obtain a thick and large-section ductile iron casting.
[0032] Application Example 3 Application Example 3 provides a method for preparing a thick and large-section ductile iron casting, comprising the following steps: High-quality scrap steel, Q10 pig iron and recycled materials are added to a coreless medium-frequency induction furnace in sequence for smelting. After all the raw materials are melted, the slag is scraped off, the composition of the molten iron is adjusted, and the in-mold inoculant block in Example 3 is placed in the pouring box to obtain a thick and large-section ductile iron casting.
[0033] Application Example 4 Application Example 4 provides a method for preparing a thick and large-section ductile iron casting, comprising the following steps: High-quality scrap steel, Q10 pig iron and recycled materials are added to a coreless medium-frequency induction furnace in sequence for smelting. After all the raw materials are melted, the slag is scraped off, the composition of the molten iron is adjusted, and the in-mold inoculant block in Example 4 is placed in the pouring box to obtain a thick and large-section ductile iron casting.
[0034] Application Example 5 Application Example 5 provides a method for preparing a thick and large-section ductile iron casting, comprising the following steps: High-quality scrap steel, Q10 pig iron and recycled materials are added to a coreless medium-frequency induction furnace in sequence for smelting. After all the raw materials are melted, the slag is scraped off, the composition of the molten iron is adjusted, and the inoculant block in Example 5 is placed in the pouring box to obtain a thick and large-section ductile iron casting.
[0035] Application Example 6 Application Example 6 provides a method for preparing a thick and large-section ductile iron casting, comprising the following steps: High-quality scrap steel, Q10 pig iron and recycled materials are added to a coreless medium frequency induction furnace in sequence for smelting. After all the raw materials are melted, the slag is scraped off, the composition of the molten iron is adjusted, and the in-mold inoculant block in Comparative Example 1 is placed in the pouring box to obtain thick and large-section ductile iron castings.
[0036] Performance testing: According to GB / T34904-2017 "Ultrasonic testing of ductile iron castings", thick and large-section ductile iron castings in various applications are tested to obtain tensile strength, yield strength, elongation and Brinell hardness.
[0037] Table 1 Performance test results of cast iron parts Combining Application Example 1 and Application Example 6, the strength and hardness of the cast iron parts in Application Example 1 are both relatively high. It can be seen that the use of the inoculant in the present application has a high aluminum content, which can promote graphitization, reduce the tendency of white cast iron, improve the morphology and distribution of graphite, increase the number of eutectic clusters, and refine the matrix structure, thereby improving the strength and hardness of the final casting.
[0038] Combined with Application Examples 1-3, the strength and hardness of the cast iron parts in Application Example 2 are the highest. It can be seen that when preparing the inoculant block and adding materials, the ratio of the raw materials ferrosilicon, calcium silicon, and aluminum ingots for remelting in Example 2 is optimal, so that the strength and hardness of the cast iron parts obtained in Application Example 2 are relatively high.
[0039] Combining Application Example 2, Application Example 4 and Application Example 5, the strength and hardness of the cast iron parts in Application Example 4 are the highest. It can be seen that when preparing the inoculant block and smelting the raw materials, the smelting conditions in Example 4 are the best, so that the strength and hardness of the cast iron parts obtained in Application Example 4 are relatively high.
[0040] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed. However, as long as it is within the scope of the claims of the present application, it shall be protected by the patent law.
Claims
1. An in-mold inoculant for preparing thick and large-section ductile iron castings, characterized in that: The inoculant comprises the following components in weight percentage: 70-80% silicon, 0.5-1.5% calcium, 3.2-4.5% aluminum, and the balance iron.
2. The in-mold inoculant for preparing thick and large-section ductile iron castings according to claim 1, characterized in that: The raw materials of the inoculant include ferrosilicon, calcium silicon and aluminum ingots for remelting.
3. The in-mold inoculant for preparing thick and large-section ductile iron castings according to claim 2, characterized in that: The weight ratio of the ferrosilicon, the calcium silicon and the aluminum ingot for remelting is 100:(2-3):(4-5).
4. The in-mold inoculant for preparing thick and large-section ductile iron castings according to claim 1, characterized in that: The inoculant is in the shape of a rectangular platform.
5. A process for preparing an in-mold inoculant block for preparing thick and large-section ductile iron castings according to any one of claims 1 to 4, characterized in that: The following steps are involved: Ingredients: crush ferrosilicon, calcium silicon and aluminum ingots for remelting respectively and set aside; Charging: First add ferrosilicon and calcium silicon into the electric furnace, and then add aluminum ingots for remelting into the electric furnace; Melting: After the charge is put into the furnace, the power can be increased for melting. The raw materials in the furnace are heated until they are melted, and then stirred to remove the scum. After confirming that there is no raw material, the furnace can be taken out to obtain the inoculant melt; Pouring: reduce the current of the electric furnace, tilt the furnace under the protection of nitrogen, pour the inoculant melt into the inoculant metal mold to obtain the inoculant rough material; Cleaning: Wait for the rough material of the inoculant to cool down completely before taking it out, and clean the gate, runner and other parts to get the finished inoculant.
6. A process for preparing an in-mold inoculant block for preparing thick and large-section ductile iron castings according to claim 5, characterized in that: In the batching step, the particle sizes of the ferrosilicon and the calcium silicon are 5-20 mm, and the aluminum ingot for remelting is a block of 50×50×50 mm.
7. A process for preparing an in-mold inoculant block for preparing thick and large-section ductile iron castings according to claim 6, characterized in that: In the smelting step, the power is 100-200kw, the voltage is 300-500V, and the current is 240-450A.
8. A process for preparing an in-mold inoculant block for preparing thick and large-section ductile iron castings according to claim 7, characterized in that: During the pouring step, the current of the electric furnace is reduced to 0A.
9. A thick and large-section ductile iron casting, characterized in that: The cast iron part is made from the in-mold inoculant block for preparing thick and large-section ductile iron castings as described in any one of claims 1 to 4.
10. A thick and heavy section ductile iron casting according to claim 9, characterized in that: The cast iron part comprises the following components in weight percentage: C accounts for 3.3-3.7%; Si accounts for 2.8-3.7%; Mn≤0.3%; P≤0.05%; S≤0.02%; Cu≤0.1%; Mg accounts for 0.04-0.06%; RE accounts for 0.01-0.03%.