Method for cold deformation of austenitic steel

By using TWIP or TRIP hardening effect and thickness thinning during the cold deformation of austenitic steel, the high strength and high ductility areas of flexible rolled materials are achieved, and the area problem that cannot be achieved in the prior art is solved. , improves load bearing capacity and work hardening effect, suitable for multi-material design and customized products.

CN119040745APending Publication Date: 2024-11-29OUTOKUMPU OY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411163708.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2016-09-29
Filing Date
2017-09-29
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The prior art cannot achieve different mechanical and physical properties in flexible rolled blanks, resulting in the inability to produce areas with different strengths and ductility in the molding process, and lack of strength and elongation for the thickness of the austenite material. Effective use.

Method used

By utilizing the TWIP or TRIP hardening effect during the cold deformation of austenitic steel, combining thickness thinning and local changes in the mechanical properties of the material, the thickness, yield strength, tensile strength and elongation are achieved in the longitudinal or transverse direction. The cold rolling process uses the cold rolling process to make the material have different mechanical properties in different regions, and achieves high strength and high ductility of the material through specific chemical composition and microstructure structure.

Benefits of technology

It realizes areas with different mechanical properties in austenitic steel products, improves the load bearing capacity and work hardening effect of the material, avoids subsequent heat treatment and galvanizing steps, reduces cost and production complexity, and is suitable for multiple materials. Design and customize products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040745A_ABST
    Figure CN119040745A_ABST
Patent Text Reader

Abstract

The invention relates to a method for local hardening of austenitic steel by utilizing the TWIP (Twin Induced Plasticity), TWIP / TRIP or TRIP (Transformation Induced Plasticity) hardening effect during cold deformation. 2, 3 ') of the material (1, 11) to be deformed having a degree of formation (Phi) in the range of 5 < = Phi < = 60%; 12) in order to achieve, in the material (1, 11), at least two contiguous regions (5, 7; 12) having different mechanical values in terms of thickness, yield strength Rp0.2, tensile strength Rm and elongation. 14, 16) has a ratio (r) between the limit load ratio [Delta] F and the thickness ratio [Delta] t in the range of 1.0 gt, rgt, 2.0 and passes through the transition region (6; 15) mechanically connecting the regions to one another, the transition region (6; the thickness of the first region (5, 14) in the deformation direction (4, 13) can be changed from the thickness (t1, t3) of the first region (5, 14) in the deformation direction (4, 13) to the thickness (t2, t4) of the second region (7, 16) in the deformation direction (4, 13).
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of an invention patent application with an application date of September 29, 2017, an application number of 201780068609.4 and an invention name of “Method for cold deformation of austenitic steel”.

[0002] The present invention relates to a method for cold deformation of austenitic steels by utilizing the TWIP (Twinning Induced Plasticity), TWIP / TRIP or TRIP (Transformation Induced Plasticity) hardening effect in the steel during deformation in order to have regions with different values ​​of mechanical and / or physical properties in the deformed steel product.

[0003] In the manufacture of transportation systems, especially car bodies and rail vehicles, engineers use arrangements to have the right material in the right place. Such possibilities are called "multi-material design" or "custom products" such as flexible rolled blanks, which are metal products with different material thicknesses along its length before stamping features and which can be cut to produce a single initial blank. Flexible rolled blanks are used in collision-related components such as pillars, transverse and longitudinal members for automotive parts. In addition, rail vehicles use flexible rolled blanks in side walls, roofs or connectors, and buses and trucks also apply flexible rolled blanks. But in the prior art, "the right material" for flexible rolled blanks only means having the right thickness in the right place, because during the flexible rolling process mechanical properties such as tensile strength will be maintained at the same value as well as thickness, tensile strength R between the flexible rolled area and the unrolled area. m The ratio of the limit load F to the product of the material width. Therefore, it is not possible to produce regions with different strength and ductility for subsequent forming processes. Usually a subsequent recrystallization annealing process and a galvanizing step follow the original flexible rolling or eccentric rolling process.

[0004] Generally speaking, DE patent application 10041280 and EP patent application 1074317 are the original patents for flexible rolled blanks. They describe a manufacturing method and an apparatus to manufacture metal strips with different thicknesses. The way to achieve this is to use an upper roll and a lower roll and to change the roll gap. However, DE patent application 10041280 and EP patent application 1074317 do not describe anything about the influence of thickness on strength and elongation and about the relationship between strength, elongation and thickness. In addition, the materials required for this relationship are not described, because no austenitic material is described.

[0005] US publication 2006033347 describes flexible rolled blanks for use in many automotive concepts and the use of sheet materials with different thicknesses. In addition, US publication 2006033347 describes the necessary sheet thickness curves that make sense for different components. However, there is no description of the influence on strength and elongation, the relationship between strength, elongation and thickness, and the materials required for this relationship.

[0006] WO publication 2014 / 202587 describes a manufacturing method for producing automotive parts using variable thickness strips. WO publication 2014 / 202587 relates to the use of press-hardenable martensitic low-alloyed steels such as 22MnB5 for hot forming schemes. However, the relationship between mechanical and technical values ​​and thickness and austenitic materials with the specific microstructural properties described are not described.

[0007] The object of the present invention is to eliminate the drawbacks of the prior art and to achieve an improved method for cold deformation of austenitic steels by exploiting the TWIP (Twinning Induced Plasticity), TWIP / TRIP or TRIP (Transformation Induced Plasticity) hardening effect of austenitic steels during deformation in order to achieve zones with different values ​​of mechanical and / or physical properties in the austenitic steel product. The essential features of the invention are listed in the attached claims.

[0008] In the method according to the invention, a hot or cold deformed strip, sheet, plate or coil made of austenitic TWIP or TRIP / TWIP or TRIP steel with different thicknesses is used as the raw material. The thickness reduction in the further cold deformation of the raw material is combined with a specific and balanced local change in the mechanical properties of the material (such as yield strength, tensile strength and elongation). The further cold deformation is carried out as flexible cold rolling or as eccentric cold rolling. The thickness of the material is variable along one direction, especially in the direction of the longitudinal extension of the material corresponding to the direction of the cold deformation of the steel. Using the method of the invention, the cold-deformed material has the desired thickness and the desired strength at that part of the deformation product when necessary. This is based on the relationship between strength, elongation and thickness. The present invention therefore takes advantage of the benefits of flexible or eccentric cold-rolled materials and solves the shortcomings of having only uniform mechanical values ​​of the prior art on fully deformed materials.

[0009] In the method of the present invention, the material is cold deformed by cold rolling so as to achieve in the material at least two regions having different specific relationships between thickness, yield strength, tensile strength and elongation in the longitudinal and / or transverse direction of the cold deformed material. Advantageously, these regions are brought into contact with each other through a longitudinal and / or transverse transition region between these regions. The limit load F1 before deformation and the limit load F2 after deformation are determined for the material in a continuous region with different mechanical values ​​before or after the transition region using the following formula:

[0010] F1 = R m1 * w *t1 (1)

[0011] and

[0012] F2 = R m2 * w *t2 (2)

[0013] Where t1 and t2 are the thickness of the area before and after cold rolling, R m1 and R m2 is the tensile strength of the region before and after cold rolling and w is the width of the material. Keeping the material width w as a constant factor, the limiting load ratio ΔF in percentage between thicknesses t1 and t2 is

[0014] ΔF = (F2 / F1)*100 (3)

[0015] and the thickness ratio Δt in percentage between loads F1 and F2 is

[0016] Δt = (t2 / t1)*100 (4).

[0017] Then the ratio r between ΔF and Δt is

[0018] r = ΔF / Δt = R m2 / R m1 (5)

[0019] In addition, the ratio r is determined in percentage between the ratio r and the degree of forming (Φ) using the following formula: Φ :

[0020] r Φ = (r / Φ)*100 (6).

[0021] According to the invention, the ratio r in the steel between the cold-rolled area and the unrolled area is in the range of 1.0>r>2.0, preferably 1.15>r>1.75, and the limit load ratio ΔF between the thickness in the unrolled area and the cold-rolled area is greater than 100% in percentage. In addition, the forming degree Φ is in the range of 5≤Φ≤60, preferably 10≤Φ≤40, and the ratio rΦ Greater than 4.0.

[0022] For cold rolled material with different thicknesses according to the invention, the maximum tolerable load is designed for each thickness region. For the prior art process with annealed material, the thickness is the only influencing variable, considering that the width is constant across the entire coil, and the tensile strength is also the same due to the annealing conditions. In the case of different work hardening levels, the tensile strength R m According to the invention, the second influencing variable and equations (1) and (2) can be transformed into equation (5). Equation (3) shows the force ratio using different thickness areas and the ratio r using equation (5) which can be related to the thickness t and the tensile strength R m For the rolled material manufactured by the present invention, the ratio r should be between 1.0>r>2.0, preferably between 1.15>r>1.75. This means that for the material used in the present invention, it is possible that the lower thickness areas can withstand higher loads. The effect of increasing the work hardening exceeds the effect of reducing the thickness. As a result of the present invention, for formula (3), the value ΔF should be ≥100% each time.

[0023] Another way to describe the materials manufactured using the present invention can be given by using equation (6), in which the relationship between the material-specific forming degree Φ and the ratio r from equation (5) is indicated. The forming degree is a deformation parameter that generally describes the continuous geometric shape change of the part during the forming process. Therefore, the relationship of equation (6) can be used as an indication of how much effort must be investigated to achieve further strength benefits. For the present invention, r Φ It should be ≥ 4.0, otherwise the effort to obtain better load values ​​is uneconomical.

[0024] The cold-formed products according to the invention can be further cut into sheets, plates, slit strips or delivered directly as coils or strips. Depending on the target use, these semi-finished products can be further processed as pipes or as another desired shape.

[0025] An advantage of the invention is that the cold deformed TWIP or TRIP / TWIP or TRIP steel combines areas with high strength and reduced thickness and areas with higher thickness and better ductility on the other hand. Thus, the invention is distinguished from other flexible rolled stock products of the prior art by combining thickness reduction with specific and balanced local changes in the mechanical properties of the sheet, plate or coil by the cold rolling process. Energy-intensive and cost-intensive heat treatments such as press hardening are therefore not necessary.

[0026] The invention makes it possible to achieve flexible rolling or eccentric rolling of materials in such a way that locally more ductile and thicker regions are available, in which the material can be thinned and hardened at the same time. On the other hand, for component regions such as the bottom of a deep-drawn component, there are high-strength and thin regions, in which hardening effects and thinning cannot usually be achieved due to the too low degree of deformation during the deep-drawing process.

[0027] Materials that can be used to produce the relationship between strength, elongation and thickness have the following conditions:

[0028] Steels with an austenitic microstructure and TWIP, TRIP / TWIP or TRIP hardening effect,

[0029] steels that are cold worked and hardened during their manufacture,

[0030] steel having a manganese content of between 10 and 25% by weight, preferably between 14 and 20% by weight,

[0031] Stainless steels having specified microstructural effects and having a nickel content ≤ 4.0 wt. %,

[0032] steels alloyed with interstitially separated nitrogen and carbon atoms having a (C+N) content between 0.4 and 0.8 wt. %,

[0033] ·With a range between 18 and 30 mJ / m 2 Between, preferably between 20 and 30 mJ / m 2 The defined stacking fault energy of the TWIP steel between 2 and 3 makes the effect reversible while maintaining a stable fully austenitic microstructure.

[0034] ·With stacking fault energy 10-18mJ / m 2 TRIP steel.

[0035] Austenitic TWIP steels can be stainless steels with more than 10.5 wt. % chromium and characterized by the alloying system CrMn or in particular CrMnN. Such alloying systems are also characterized in particular by a low nickel content (≤ 4 wt. %) to reduce material costs and the costs of producing non-volatile components in multi-year production series. A useful chemical composition contains, in wt. %, 0.08-0.30% carbon, 14-26% manganese, 10.5-16% chromium, less than 0.8% nickel and 0.2-0.8% nitrogen.

[0036] Austenitic TRIP / TWIP stainless steels may be stainless steels having the alloying system CrNi (e.g. 1.4301 or 1.4318), CrNiMn (e.g. 1.4376) or CrNiMo (e.g. 1.4401). Likewise, ferritic austenitic duplex TRIP / TWIP stainless steels (e.g. 1.4362 and 1.4462) are beneficial for the method of the invention.

[0037] 1.4301 austenitic TRIP / TWIP stainless steel contains, by weight, less than 0.07% carbon, less than 2% silicon, less than 2% manganese, 17.50-19.50% chromium, 8.0-10.5% nickel, less than 0.11% nitrogen, the balance being iron and unavoidable impurities occurring in stainless steel. 1.4318 austenitic TRIP / TWIP stainless steel contains, by weight, less than 0.03% carbon, less than 1% silicon, less than 2% manganese, 16.50-18.50% chromium, 6.0-8.0% nickel, 0.1-0.2% nitrogen, the balance being iron and unavoidable impurities occurring in stainless steel. 1.4401 austenitic TRIP / TWIP stainless steel contains, by weight%, less than 0.07% carbon, less than 1% silicon, less than 2% manganese, 16.50-18.50% chromium, 10.0-13.0% nickel, 2.0-2.5% molybdenum, less than 0.11% nitrogen, the remainder being iron and unavoidable impurities occurring in stainless steel.

[0038] 1.4362 ferritic austenitic duplex TRIP / TWIP stainless steel contains, by weight, less than 0.03% carbon, less than 1% silicon, less than 2% manganese, 22.0-24.0% chromium, 4.5-6.5% nickel, 0.1-0.6% molybdenum, 0.1-0.6% copper, 0.05-0.2% nitrogen, the balance being iron and unavoidable impurities occurring in stainless steel. 1.4462 ferritic austenitic duplex TRIP / TWIP stainless steel contains, by weight, less than 0.03% carbon, less than 1% silicon, less than 2% manganese, 22.0-24.0% chromium, 4.5-6.5% nickel, 2.5-3.5% molybdenum, 0.10-0.22% nitrogen, the balance being iron and unavoidable impurities occurring in stainless steel.

[0039] With austenitic stainless materials, further surface coating is not necessary. In the case of the material being used for components for vehicles, standard electrophoretic coating of the body is sufficient. This is particularly beneficial for wet corrosive parts, with combined advantages in terms of cost, production complexity and corrosion protection.

[0040] With TWIP or TRIP / TWIP stainless steel, it is also possible to avoid the subsequent galvanizing process after the flexible cold rolling process or the eccentric cold rolling process. With reference to the known properties of stainless steel, the final cold rolled material has improved properties in terms of non-scaling and heat resistance. Therefore, the cold rolled material of the present invention can be used in high temperature solutions.

[0041] The benefit for fully austenitic TWIP steels is the non-magnetic properties under conditions such as forming or welding. Therefore, fully austenitic TWIP steels are suitable for application as flexible rolled stock in battery electric vehicle components.

[0042] The invention describes a manufacturing method for rolling different regions into coils or strips, wherein

[0043] ·Production width: 650≤t≤1600mm

[0044] · Initial thickness: 1.0≤t≤4.5mm

[0045] • Intermediate annealing during deformation and annealing after deformation can be used to obtain uniform material properties.

[0046] Component to be manufactured according to the invention

[0047] Auto parts such as airbag bushings, auto body parts such as chassis parts, subframes, pillars, cross members, guide channels, rocker rails,

[0048] · are commercial vehicle parts in the form of semi-finished sheets, tubes or profiles,

[0049] · Rail vehicle components with a continuous length ≥ 2000 mm such as side walls, floors, roofs,

[0050] · Tubes made from strip or slit strip,

[0051] ·Vehicle additional parts such as collision-related door side anti-collision beams,

[0052] ·It is a non-magnetic component used in battery electric vehicles,

[0053] ·It is a roll-formed or hydroformed part for transportation applications.

[0054] The present invention will be described in more detail with reference to the following drawings, in which

[0055] Figure 1 shows a preferred embodiment of the invention shown diagrammatically and viewed as an axonometric projection,

[0056] Figure 2Another preferred embodiment of the invention is shown diagrammatically and viewed as an axonometric projection.

[0057] exist Figure 1 A TWIP material block 1 is flexibly cold rolled along a rolling direction 4 on both an upper surface 2 and a lower surface 3. The material block 1 has a first region 5, where the material is thick and the material is relatively ductile and hardened at the same time. The material block also has a transition region 6, where the material thickness can vary so that the thickness decreases from the first region 5 to a second region 7, where the material has a higher strength but a lower ductility.

[0058] exist Figure 2 The TWIP material block 11 is flexibly cold rolled only on the upper surface 12 along the rolling direction 13. Figure 1 As in the embodiment of the present invention, the material block 11 has a first region 14 in which the material is thick and the material is relatively ductile and hardened at the same time. The material block 11 also has a transition region 15 in which the material thickness can vary so that the thickness decreases from the first region 14 to a second region 16 in which the material has a higher strength but a lower ductility.

[0059] The method according to the invention was tested using a TWIP (Twinning Induced Plasticity) austenitic steel having the chemical composition in wt. % in Table 1 below.

[0060] alloy Cr Mn Ni C N A(Melt 1) 16 18 ≤2 0.3 0.4 B(Melt 2) 14 15 ≤2 0.3 0.6 C (melt 3) 12 20 ≤2 0.08 - D (melt 4) 6 14 0.5 0.08 0.2 E(melt 5) 18 6 2.5 0.06 -

[0061] Table 1

[0062] Alloys AC and E are austenitic stainless steels, while alloy D is an austenitic steel.

[0063] The yield strength R of each alloy AE was completed before and after flexible cold rolling. p0.2 , tensile strength R m and elongation A 80 The alloy was rolled on both the upper and lower surfaces in the flexible cold rolling. The measurement results are described in Table 2 below as well as the initial thickness and the resulting thickness.

[0064]

[0065] Table 2

[0066] The results in Table 2 show that the yield strength Rp during flexible rolling 0.2 and tensile strength R m Generally improved, while the elongation A during flexible rolling 80 Generally reduced.

[0067] The method according to the invention was also tested using TRIP (Transformation Induced Plasticity) or TRIP / TWIP austenitic or ferritic-austenitic dual-phase standardized steels having the chemical composition in wt. % in Table 3 below.

[0068] Brand Cr Mn Ni C Mo N 1.4301 18 1.2 8.0 0.04 - - 1.4318 17 1.0 7.5 0.02 - 0.14 1.4362 22 1.3 3.8 0.02 - 0.10 1.4401 17 1.2 10.5 0.02 2.2 - 1.4462 22 1.4 5.8 0.02 3.0 0.17

[0069] Table 3

[0070] In Table 3, grades 1.4362 and 1.4462 are ferritic austenitic duplex stainless steels, and the others 1.4301, 1.4318 and 1.4401 are austenitic stainless steels.

[0071] Before and after flexible rolling, the mechanical values, yield strength Rp and 0.2 , tensile strength R m and elongation, and the results are described in Table 4 below along with the initial thickness before flexible rolling and the resulting thickness after flexible rolling.

[0072]

[0073] Table 4

[0074] The results in Table 4 show that in addition to austenitic TWIP stainless steels, duplex TRIP or TWIP / TRIP stainless steels with an austenite content greater than 40 vol. %, preferably greater than 50 vol. %, also have high suitability for the hardening zone in the flexible rolling process.

[0075] The influence of the forming degree Φ was tested for TWIP, TWIP / TRIP and TRIP steels according to the invention. Table 5 shows the results for the low nickel austenitic stainless steel B of Table 1 .

[0076]

[0077] Table 5

[0078] Table 6 shows the results for austenitic stainless steel 1.4318

[0079]

[0080] Table 6

[0081] Table 7 shows the results for the duplex austenitic ferritic stainless steel 1.4362.

[0082]

[0083] Tables 7 and 8 show the results for the duplex austenitic ferritic stainless steel 1.4462.

[0084]

[0085] Tables 8 and 9 show the results for austenitic stainless steel 1.4301.

[0086]

[0087] Table 9.

Claims

1. A method for local hardening of austenitic steel by utilizing the TWIP (twinning induced plasticity), TWIP / TRIP or TRIP (transformation induced plasticity) hardening effect during cold deformation, characterized in that cold deformation is carried out by cold rolling on at least one surface (2, 3; 12) of a material to be deformed (1, 11) with a forming degree (Φ) in the range of 5 ≤ Φ ≤ 60%, so as to achieve in the material (1, 11) a change in thickness, yield strength R p0.2 , tensile strength R m At least two consecutive regions (5, 7; 14, 16) with different mechanical values ​​in terms of mechanical load ratio ΔF and elongation have a ratio (r) between a limit load ratio ΔF and a thickness ratio Δt in the range of 1.0>r>2.0, and the regions (5, 7; 14, 16) are mechanically connected to each other via a transition region (6; 15), wherein the thickness can be changed from a thickness (t1, t3) of a first region (5, 14) in the deformation direction (4, 13) to a thickness (t2, t4) of a second region (7, 16) in the deformation direction (4, 13).

2. The method according to claim 1, characterized in that the cold rolling is performed by flexible cold rolling.

3. The method according to claim 1, characterized in that the cold rolling is performed by eccentric cold rolling. 4 . The method according to claim 1 , wherein the degree of forming (Φ) is in the range of 10≤Φ≤40% and the ratio (r) is in the range of 1.15>r>1.

75.

5. The method according to claims 1-4, characterized in that the material to be deformed is an austenitic TWIP material.

6. The method according to claim 5, characterized in that the material to be deformed is austenitic stainless steel.

7. The method according to claims 1-4, characterized in that the material to be deformed is a TRIP / TWIP material.

8. The method according to claim 7, characterized in that the material to be deformed is austenitic duplex stainless steel.

9. The method according to claim 7, characterized in that the material to be deformed is a ferritic austenitic duplex stainless steel containing more than 40% by volume of austenite, preferably more than 50% by volume of austenite.

10. The method according to claims 1-4, characterized in that the material to be deformed is a TRIP material.

11. Use of a cold rolled product produced according to claim 1 having different mechanical values ​​deformed in at least two consecutive regions (5, 7; 14, 16) with a forming degree (Φ) in the range of 5≤Φ≤60% and having a ratio (r) between the limit load ratio ΔF and the thickness ratio Δt in the range of 1.0>r>2.0 as an automotive component, airbag bushing, automotive body component such as chassis parts, subframes, pillars, cross members, guide channels, rocker rails.

12. Use of a cold-rolled product produced according to claim 1 having different mechanical values ​​deformed in at least two consecutive regions (5, 7; 14, 16) with a forming degree (Φ) in the range of 5≤Φ≤60% and having a ratio (r) between the limit load ratio ΔF and the thickness ratio Δt in the range of 1.0>r>2.0 as a commercial vehicle component with semi-finished sheets, tubes or profiles, such as rail vehicle components with a continuous length ≥2000 mm, such as side walls, floors, roofs.

13. Use of a cold rolled product produced according to claim 1 having different mechanical values ​​deformed in at least two consecutive regions (5, 7; 14, 16) with a forming degree (Φ) in the range of 5≤Φ≤60% and having a ratio (r) between the limit load ratio ΔF and the thickness ratio Δt in the range of 1.0>r>2.0 as a tube produced from a strip or a slit strip.

14. Use of a cold-rolled product produced according to claim 1 having different mechanical values ​​deformed in at least two consecutive regions (5, 7; 14, 16) with a forming degree (Φ) in the range of 5≤Φ≤60% and having a ratio (r) between the limit load ratio ΔF and the thickness ratio Δt in the range of 1.0>r>2.0 as a vehicle additional part, such as a crash-related door side impact beam.

15. Use of a cold rolled product produced according to claim 1 having different mechanical values ​​deformed in at least two consecutive regions (5, 7; 14, 16) with a forming degree (Φ) in the range of 5 ≤ Φ ≤ 60% and having a ratio (r) between the limit load ratio ΔF and the thickness ratio Δt in the range of 1.0>r>2.0 as a component with non-magnetic properties for battery electric vehicles.

16. Use of a cold rolled product produced according to claim 1 having different mechanical values ​​deformed in at least two consecutive regions (5, 7; 14, 16) with a forming degree (Φ) in the range of 5≤Φ≤60% and having a ratio (r) between the limit load ratio ΔF and the thickness ratio Δt in the range of 1.0>r>2.0 as a roll-formed or hydroformed component for transportation applications.