Coating-free super weathering steel and manufacturing method thereof
Through the synergistic action of alloy elements such as Cu, Cr, P and microalloyation of niobium and titanium, combined with the controlled rolling and cooling technology, the problem of poor rust layer stability in existing super weathering steels in severe corrosion environments has been solved, and high The coating-free super weather-resistant steel with strength, high toughness and good corrosion resistance meets the needs of high strength, lightweight and low carbon development.
Patent Information
- Application Number
- CN202411174863.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-29
AI Technical Summary
Existing super weathering steels are difficult to form stable rust layers in severe corrosion environments, resulting in poor corrosion resistance and difficult to achieve coating-free use. At the same time, the high alloy system is not conducive to the economics of steel plates and is not strong enough to meet the high-strength and lightweighting. , low-carbon development needs.
Through the synergistic action of alloy elements such as Cu, Cr, and P, combined with niobium and titanium microalloyation and rolling and cooling control processes, the stability of the rust layer is improved, the strength and toughness of the steel are improved, and high yield strength and tensile strength are prepared. And good corrosion resistance properties of coating-free super weather-resistant steel.
It realizes coating-free use in severe corrosion environments, significantly improving corrosion resistance and economicality. The yield strength and tensile strength of steel reach 420~750MPa and 520~860MPa, and the corrosion rate is lower than 40% of Q355 steel. , and obtain fine polygonal ferrite structure.
Smart Images

Figure CN119040764A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of atmospheric corrosion resistant steel, and specifically relates to a coating-free super weathering steel and a manufacturing method thereof. Background Art
[0002] Weathering steel is made by adding a small amount of copper, chromium, nickel, molybdenum and other alloy elements to ordinary carbon steel. While ensuring its mechanical properties, this steel has a corrosion resistance that is 2 to 8 times that of ordinary carbon steel, and its corrosion resistance increases more significantly over time. After several years of service in the atmospheric environment, a stable and dense rust layer forms on the surface of the weathering steel, which can slow down the corrosion of the substrate and achieve paint-free use. The use of weathering steel without painting can greatly save painting costs, is environmentally friendly, and shortens the construction period. At the same time, it greatly reduces the maintenance cost of the steel during use, which is of great significance.
[0003] Studies have shown that the rust layer stabilization process of weathering steel is related to the chemical composition, use environment and structure of the steel. In areas without severe atmospheric pollution or not particularly humid, weathering steel can gradually form a stable rust layer and can be directly exposed to the atmosphere. However, in heavily polluted areas, coastal areas and other harsh corrosive environments, it is difficult for ordinary weathering steel to form a stable rust layer, and super weathering steel must be used to achieve paint-free use. In the prior art, super weathering steels mostly use high alloy systems, adding high alloy elements such as Ni and Mo, which is not conducive to the economy of steel plates. Moreover, the current highest-grade high-weathering steel is Q355GNH, and the strength level is only 355MPa, which is difficult to meet the development needs of high-strength, lightweight and low-carbon. In addition, the existing super weathering steel still has the problem of poor rust layer stability, poor corrosion resistance in harsh corrosive environments, and difficulty in paint-free use in the early stage of use. Therefore, it is necessary to develop super weathering steel that takes into account both economy and corrosion resistance to achieve paint-free use in harsh corrosive environments. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a painting-free super weathering steel and a manufacturing method thereof in view of the shortcomings of the prior art. The synergistic effect of alloying elements such as Cu, Cr, and P is used to improve the stability of the rust layer of the weathering steel, and high strength and high toughness are obtained by combining niobium and titanium microalloying and controlled rolling and controlled cooling processes, thereby improving the economy and corrosion resistance of the super weathering steel and achieving the effect of painting-free use.
[0005] In order to solve the technical problem raised by the present invention, the present invention provides a coating-free super weathering steel, and the chemical composition of the coating-free super weathering steel includes, by mass percentage: C: 0.01-0.07%, Si: 0.20-0.80%, Mn: 0.3-0.9%, Cu: 0.15-0.25%, Cr: 1.25-1.8%, P: 0.06-0.10%, S≤0.02%, Nb: 0-0.10%, Ti: 0-0.10%, Nb+Ti: 0.05-0.12%, Cu / P: 2-4, Cr / Cu: 5-10, and the rest is Fe and unavoidable impurities.
[0006] Preferably, the chemical composition of the paint-free super weathering steel includes, by mass percentage: C: 0.01-0.07%, Si: 0.20-0.80%, Mn: 0.3-0.9%, Cu: 0.2-0.25%, Cr: 1.3-1.5%, P: 0.07-0.09%, S≤0.02%, Nb: 0-0.10%, Ti: 0-0.10%, Nb+Ti: 0.05-0.12%, Cu / P: 3-4, Cr / Cu: 6-7, and the rest is Fe and unavoidable impurities.
[0007] In the above scheme, the metallographic structure of the paint-free super weathering steel is a polygonal ferrite structure, the grain size is ≥11, and the inclusion level is ≤0.5.
[0008] In the above scheme, the yield strength R of the coating-free super weathering steel is t0.5 420~750MPa, tensile strength R m 520~860MPa, yield strength ratio R t0.5 / R m ≤0.9, elongation after break A 50mm ≥20%, -20℃ impact energy KV2≥100J.
[0009] In the above scheme, the paint-free super weathering steel is tested for corrosion resistance according to TB / T 2375-1993, and its corrosion rate is ≤1.6g / (m 2 .h), the relative corrosion rate of Q355 steel is less than 40%.
[0010] The present invention also provides a method for manufacturing a coating-free super weathering steel, comprising the following steps:
[0011] 1) Carry out converter smelting according to the chemical composition of the coating-free super weathering steel;
[0012] 2) LF refining is performed, and the S content of the molten steel after refining is ≤0.010%, and the P content is 0.06-0.1%;
[0013] 3) Perform RH vacuum treatment, vacuum degree ≤ 70Pa, vacuum cycle time ≥ 10min;
[0014] 4) Continuously casting into billets, heating the billets at a heating temperature of 1100-1250°C;
[0015] 5) rolling, the start temperature of finishing rolling is 850-950°C, and the end temperature of finishing rolling is 800-880°C;
[0016] 6) Perform laminar cooling at a cooling rate of 15 to 30°C / s and curl to obtain a coating-free super weathering steel.
[0017] In the above scheme, the rolling also includes rough rolling, the starting temperature of rough rolling is 1000-1200°C, the ending temperature of rough rolling is 880-970°C, and the total reduction rate of rough rolling is 65-85%.
[0018] In the above scheme, the cumulative reduction rate of the finish rolling is ≥70%, and the thickness of the steel plate after the finish rolling is 1.5 to 5 mm.
[0019] In the above scheme, the curling temperature is 480-600°C.
[0020] Preferably, the vacuum degree of the RH vacuum treatment is ≤50Pa, the vacuum cycle time is 15 to 30 minutes, and the vacuum end temperature is 1550 to 1650°C.
[0021] Preferably, the heating temperature of the casting is 1180-1210°C.
[0022] Preferably, the rough rolling start temperature is 1150-1180°C, and the rough rolling end temperature is 930-950°C.
[0023] Preferably, the start temperature of the finishing rolling is 890-930°C, and the end temperature of the finishing rolling is 850-880°C.
[0024] Preferably, the cooling rate of the laminar cooling is 20-25° C. / s.
[0025] The functions and mechanisms of each element in the present invention are as follows:
[0026] Carbon (C): Carbon is a basic strengthening element for steel, but too high a carbon content is harmful to the ductility and welding properties of steel. Therefore, the present invention adopts a low carbon component, and the C content is limited to 0.01-0.07%.
[0027] Silicon (Si): Silicon plays a role in deoxidation and solid solution strengthening, and the addition of silicon is beneficial to corrosion resistance, but excessive silicon will deteriorate the mechanical properties of steel. Therefore, the Si content of the present invention is limited to 0.20-0.8%.
[0028] Manganese (Mn): Manganese plays a role in solid solution strengthening, which can make up for the strength loss caused by low carbon. However, manganese easily causes structural segregation and the formation of MnS inclusions in the metallurgical process, thereby deteriorating the mechanical properties and corrosion resistance of the steel. Therefore, the Mn content of the present invention is limited to 0.3-0.9%.
[0029] Copper (Cu): Copper is a corrosion-resistant element that can significantly increase the self-corrosion potential of steel, form a copper oxide film on the surface of steel, and improve the thermodynamic stability of steel. In addition, copper can also work synergistically with chromium and phosphorus to promote the refinement of the α-FeOOH crystals of the stable rust layer component, making the rust layer dense and stable. This in turn improves the corrosion resistance of the steel. However, too high a Cu content will have an adverse effect on welding performance. When the Cu content exceeds 0.25%, problems such as thermal cracks are prone to occur during welding. By reducing the Cu content to 0.15% to 0.25%, the welding performance can be improved, and the quality and reliability of the welded joint can be improved. Reducing the Cu content can also significantly reduce production costs. Therefore, the Cu content of the present invention is limited to 0.15 to 0.25%, preferably 0.2 to 0.25%.
[0030] Chromium (Cr): Chromium is an important corrosion-resistant element. It can form a dense chromium oxide protective film on the surface of the material to prevent the invasion of corrosive media. When the Cr content is increased to more than 1.25%, the chromium element is enriched in the rust layer to form a thermodynamically stable, amorphous α-Fe 1-x Cr x OOH can significantly improve the corrosion resistance of the material, so that it has a longer service life in harsh environments such as marine atmosphere and industrial atmosphere. Cr can be solid solution strengthened and precipitation strengthened, thereby improving the strength and hardness of the material. As the Cr content increases, the strength and hardness of the material gradually increase. However, excessive chromium will reduce the toughness and welding performance of the steel. Therefore, the Cr content of the present invention is limited to 1.25-1.8%, preferably 1.3-1.5%.
[0031] Phosphorus (P): Phosphorus is a harmful element in steel, which deteriorates the toughness and weldability of steel. However, phosphorus is an effective corrosion-resistant element. Phosphoric acid can be converted into phosphates, which block cracks and holes in the rust layer and significantly improve the protectiveness of the rust layer. Phosphorus can also synergize with copper and chromium to promote the enrichment of each other in the rust layer, so that a protective barrier is formed on the surface of the steel to block the corrosive medium, thereby improving the atmospheric corrosion resistance of the steel. Therefore, the P content of the present invention is limited to 0.06-0.10%, preferably 0.07-0.09%.
[0032] In order to better exert the synergistic effect of the three elements, the Cu / P content ratio is limited to 2-4, and the Cr / Cu content ratio is limited to 5-10. This is because the two elements Cu and P have a synergistic effect, mainly by synergistically forming a protective rust film and promoting the increase of their content in the rust layer. The content ratio of the two elements is controlled at 2-4 to better exert their synergistic efficiency. Cr and Cu elements also promote each other's enrichment in the rust layer. Controlling the content ratio of the two elements at 5-10 can effectively increase the enrichment of Cr content in the rust layer.
[0033] Niobium (Nb) and titanium (Ti): Niobium and titanium are both microalloying elements that can significantly refine the grains. Only by precisely controlling the addition of Nb and Ti can the optimization of the grain structure be achieved. Fine-grained structure can improve the strength, toughness and corrosion resistance of steel. Niobium and titanium not only play the role of solid solution strengthening and precipitation strengthening in steel, but also have a synergistic strengthening effect. The solid solution strengthening of niobium can improve the strength of steel, while the precipitation strengthening of titanium can further improve the impact toughness of steel. The synergistic effect of the two makes the steel of the present invention have higher comprehensive performance. Therefore, the present invention limits the addition of the two microalloys to Nb: 0-0.10%, Ti: 0-0.10%, and limits the total addition of Nb+Ti to 0.05-0.12%. It can give full play to the role of niobium and titanium in refining grains, improving strength and toughness, and avoid the adverse effects of excessive addition of microalloys such as reducing weld impact toughness, increasing ductile-brittle transition temperature and reducing low-temperature toughness.
[0034] Sulfur (S): Sulfur is a harmful element that can react with manganese to form harmful inclusions, manganese sulfide, which not only reduces the mechanical properties of steel, but also reduces the corrosion resistance of steel. Therefore, the present invention controls the S content to ≤ 0.020%.
[0035] The technical concept of the present invention in the manufacturing method is:
[0036] In the present invention, after the molten iron is smelted in a converter, an LF furnace and an RH vacuum furnace are used for desulfurization treatment. Since a high P component system is used, the desulfurization process in steelmaking can be reduced. At the same time, the LF furnace and the RH vacuum furnace treatment can make the niobium and titanium microalloying evenly distributed in the molten steel, induce the formation of a large number of fine and dispersed non-metallic inclusions in the molten steel, which will become the core of ferrite nucleation. During the rolling process, the finishing temperature is controlled in the range of 800 to 950° C. to ensure that the carbon and nitrides of niobium and titanium are uniformly precipitated and distributed in the grains and grain boundaries. A faster cooling rate is adopted to make the steel plate quickly curled to 480 to 600° C. to prevent the ferrite structure from coarsening. The fine polygonal ferrite structure steel is obtained by combining the TMCP process with niobium and titanium microalloying, which has higher strength and toughness and can make up for the toughness loss caused by high phosphorus elements.
[0037] Compared with the prior art, the present invention has the following beneficial effects:
[0038] Most of the existing super weathering steels adopt high alloy systems, adding high Mn, Ni, Mo and other alloying elements, which is not conducive to the economy of steel plates, and the strength is low, making it difficult to meet the development trend of high strength and low carbon. In the present invention, no elements such as Ni and Mo are added, and the stability of the rust layer is improved through the synergistic effect of alloying elements such as Cu, Cr, and P, and the corrosion resistance of the steel is improved. Compared with the existing technology, the corrosion resistance is greatly improved, and the use without painting is achieved. At the same time, niobium and titanium microalloying is adopted, and the TMCP controlled rolling and controlled cooling process is used to obtain fine polygonal ferrite structure steel, which has higher strength and toughness. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 This is a metallographic structure photograph of the paint-free super weathering steel in Example 1 of the present invention.
[0040] Figure 2 This is a photo of inclusions in the paint-free super weathering steel in Example 1 of the present invention. DETAILED DESCRIPTION
[0041] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the content of the present invention is not limited to the following embodiments.
[0042] Examples 1 to 10
[0043] The chemical composition of the coating-free super weathering steel in Examples 1 to 10 is shown in Table 1.
[0044] Table 1
[0045]
[0046] Note: ① Comparative Example 1 is Q355GNH steel, and its chemical composition, in addition to that listed in the table, also includes: Ni 0.39%, Mo 0.12%, Zr 0.09%, V 0.05%; ② Comparative Example 2 is Q355GNH steel, and its chemical composition, in addition to that listed in the table, also includes: Ni 0.21%, Mo 0.27%, Zr 0.13%, V 0.07%.
[0047] The method for manufacturing the coating-free super weathering steel in Examples 1 to 10 comprises the following steps:
[0048] 1) Carry out converter smelting according to the chemical composition in Table 1;
[0049] 2) LF refining is performed, and the S content of the molten steel after refining is ≤0.010%, and the P content is 0.06-0.1%;
[0050] 3) Perform RH vacuum treatment, vacuum degree ≤ 70Pa, vacuum cycle time ≥ 10min, vacuum end temperature 1550~1650℃;
[0051] 4) Continuously casting into billets, heating the billets at a heating temperature of 1100-1250°C;
[0052] 5) rolling, the starting temperature of rough rolling is 1000-1200°C, the ending temperature of rough rolling is 880-970°C, the total reduction rate of rough rolling is 65-85%; the starting temperature of finishing rolling is 850-950°C, the ending temperature of finishing rolling is 800-880°C, the cumulative reduction rate of finishing rolling is ≥70%, and the steel plate with a thickness of 1.5-5 mm is rolled after 5-10 passes;
[0053] 6) laminar cooling is performed at a cooling rate of 15 to 30°C / s, and the steel is cooled to 480 to 600°C and curled to obtain a coating-free super weathering steel.
[0054] The main process parameters involved in the manufacturing method are shown in Tables 2-3.
[0055] Table 2
[0056]
[0057] Table 3
[0058]
[0059] The mechanical properties, metallographic structures and inclusions of the paint-free super weathering steel in Examples 1 to 10 were tested, and the results are shown in Table 4.
[0060] Table 4
[0061]
[0062]
[0063] It can be seen from Table 4 that the yield strength R t0.5 420~750MPa, tensile strength R m 520~860MPa, yield strength ratio R t0.5 / R m ≤0.9, elongation after break A 50mm ≥20%, -20℃ impact energy KV2≥100J, which is a significant improvement over the comparative example Q355GNH steel.
[0064] Figure 1 This is a photo of the metallographic structure of the paint-free super weathering steel in Example 1. It can be seen from the figure that its metallographic structure is polygonal ferrite with a grain size of 11. Figure 2This is a photo of inclusions in the paint-free super weathering steel in Example 1. It can be seen from the figure that the inclusions are Class D inclusions with a grade of 0.5. Figures 1-2 As can be seen from Table 4, the coating-free super weathering steel of the present invention obtains a fine polygonal ferrite structure steel, and its grain size and inclusion level are significantly improved compared with the comparative example Q355GNH steel.
[0065] In order to further verify the corrosion resistance of the unpainted super weathering steel, a 3-day periodic immersion corrosion test was carried out in 0.01 mol / L sodium bisulfite solution according to the TB / T 2375-1993 “Test method for periodic immersion corrosion of weathering steel for railway use” standard. The results are shown in Table 5.
[0066] Table 5
[0067]
[0068]
[0069] It can be seen from Table 5 that the corrosion rate of the coating-free super weathering steel of the present invention is ≤1.6g / (m 2 .h), the relative corrosion rate of Q355 steel is less than 40%, and it is a significant improvement over Q355GNH steel.
[0070] The above embodiments are merely examples for clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above descriptions. It is not necessary and impossible to list all the implementation methods here, and the obvious changes or modifications derived therefrom are still within the protection scope of the invention.
Claims
1. A coating-free super weathering steel, characterized in that: Its chemical composition, by mass percentage, includes: C: 0.01-0.07%, Si: 0.20-0.80%, Mn: 0.3-0.9%, Cu: 0.15-0.25%, Cr: 1.25-1.8%, P: 0.06-0.10%, S≤0.02%, Nb: 0-0.10%, Ti: 0-0.10%, Nb+Ti: 0.05-0.12%, Cu / P: 2-4, Cr / Cu: 5-10, and the rest is Fe and unavoidable impurities.
2. The coating-free super weathering steel according to claim 1, characterized in that: Its chemical composition, by mass percentage, includes: C: 0.01-0.07%, Si: 0.20-0.80%, Mn: 0.3-0.9%, Cu: 0.2-0.25%, Cr: 1.3-1.5%, P: 0.07-0.09%, S≤0.02%, Nb: 0-0.10%, Ti: 0-0.10%, Nb+Ti: 0.05-0.12%, Cu / P: 3-4, Cr / Cu: 6-7, and the rest is Fe and unavoidable impurities.
3. The coating-free super weathering steel according to claim 1, characterized in that: The metallographic structure of the paint-free super weathering steel is a polygonal ferrite structure, the grain size is ≥11, and the inclusion level is ≤0.
5.
4. The coating-free super weathering steel according to claim 1, characterized in that: The yield strength R of the coating-free super weathering steel t0.5 420~750MPa, tensile strength R m 520~860MPa, yield strength ratio R t0.5 / R m ≤0.9, elongation after break A 50mm ≥20%, -20℃ impact energy KV2≥100J.
5. The coating-free super weathering steel according to claim 1, characterized in that: The corrosion resistance of the paint-free super weathering steel is tested according to TB / T 2375-1993, and its corrosion rate is ≤1.6g / (m 2 .h), the relative corrosion rate of Q355 steel is less than 40%.
6. A method for manufacturing the coating-free super weathering steel according to any one of claims 1 to 5, characterized in that: The steps include: 1) Carry out converter smelting according to the chemical composition of the coating-free super weathering steel; 2) LF refining is performed, and the S content of the molten steel after refining is ≤0.010%, and the P content is 0.06-0.1%; 3) Perform RH vacuum treatment, vacuum degree ≤ 70Pa, vacuum cycle time ≥ 10min; 4) Continuously casting into billets, heating the billets at a heating temperature of 1100-1250°C; 5) rolling, the starting temperature of rough rolling is 1000-1200°C, the ending temperature of rough rolling is 880-970°C, the starting temperature of finish rolling is 850-950°C, and the ending temperature of finish rolling is 800-880°C; 6) Perform laminar cooling at a cooling rate of 15 to 30°C / s and curl to obtain a coating-free super weathering steel.
7. The method for manufacturing the coating-free super weathering steel according to claim 6, characterized in that: The vacuum degree of the RH vacuum treatment is ≤50Pa, the vacuum cycle time is 15 to 30 minutes, and the vacuum end temperature is 1550 to 1650°C.
8. The method for manufacturing the coating-free super weathering steel according to claim 6, characterized in that: The total reduction rate of the rough rolling is 65-85%, the cumulative reduction rate of the finish rolling is ≥70%, and the thickness of the steel plate after the finish rolling is 1.5-5 mm.
9. The method for manufacturing the coating-free super weathering steel according to claim 6, characterized in that: The heating temperature of the casting is 1180-1210°C; the starting temperature of the rough rolling is 1150-1180°C, and the ending temperature of the rough rolling is 930-950°C; the starting temperature of the finish rolling is 890-930°C, and the ending temperature of the finish rolling is 850-880°C.
10. The method for manufacturing the coating-free super weathering steel according to claim 6, characterized in that: The cooling rate of the laminar cooling is 20-25°C / s; the curling temperature is 480-600°C.
Citation Information
Patent Citations
Marine atmosphere corrosion resistant high-strength steel and production method thereof
CN114908298A
Titanium-containing weathering steel for low-cost 650MPa-grade photovoltaic support and preparation method of titanium-containing weathering steel
CN116219307A
Industrial atmospheric corrosion resistant high-strength steel and production method thereof
CN116463553A
Economical weathering steel with yield strength larger than or equal to 690 MPa and production method
CN116516248A
Weathering resistant steel not prone to rusting and production method thereof
CN118166282A
Cited By
Desert-climate-resistant coating-free weathering steel and preparation method thereof
CN119571208A
Hot-rolled wire rod and red rust control production process
CN119956250A
A hot-rolled wire rod and a production process for red rust control
CN119956250B
Thick 650MPa-grade high-toughness hot-rolled weather-resistant steel plate and preparation method thereof
CN120818662A
Thick 700MPa-grade high-toughness hot-rolled weather-resistant steel plate and preparation method thereof