Alloy coating and preparation method and application thereof

By preparing TiAlCrNbRe antioxidant coating on the surface of TiAl alloy, using multi-arc ion plating and deposition technology and the addition of appropriate elements, the compatibility and stability problems between the existing coating and TiAl alloy at high temperatures were solved, significantly improving the quality of the existing coating. The high-temperature oxidation resistance and interface bonding strength of the alloy are provided.

CN119040814APending Publication Date: 2024-11-29SHANGHAI INST OF CERAMIC CHEM & TECH CHINESE ACAD OF SCI
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411156512.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The chemical composition differences between the existing antioxidant coatings and TiAl alloys at high temperatures lead to elemental interdiffusion, coating peeling and poor interfacial stability, limiting the high-temperature oxidation resistance of TiAl alloys.

Method used

Using TiAlCrNbRe alloy as the target material, an antioxidant coating was prepared by deposition on the surface of the alloy substrate by multi-arc ionization. An appropriate amount of Al/Cr elements was added to generate a dense Al2O3 phase, and a small amount of Nb and rare earth elements were added to improve the resistance of the coating. Oxidation capacity and interface compatibility.

Benefits of technology

Good chemical compatibility with TiAl alloy is achieved, the interdiffusion between the coating is reduced, the oxidation resistance and interface bonding strength of the coating are improved, and the stability and performance in high temperature environments are ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040814A_ABST
    Figure CN119040814A_ABST
Patent Text Reader

Abstract

The invention discloses an alloy coating and a preparation method thereof. The coating comprises 15-35 at.% of Ti, 35-55 at.% of Al, 15-35 at.% of Cr, 1-10 at.% of Nb and less than or equal to 3 at.% of rare earth element Re. Wherein the rare earth element Re is at least one of Ce, Gd, Yb, Lu, Y and Hf, and the sum of the atomic percent of Ti, Al, Cr, Nb and Re is 100%. The coating is prepared by a multi-arc ion plating deposition method. The coating has the characteristics of high melting point and good chemical compatibility with matrix alloy. The invention further discloses an anti-oxidation protection application of the coating on an alloy matrix such as a TiAl alloy or a titanium alloy, the coating is high in density, no obvious mutual diffusion exists between the coating and the TiAl alloy or the titanium alloy at a high temperature, and the anti-oxidation performance of the alloy can be effectively improved. In addition, the bonding strength of the coating and the base body is high, and the use requirements of the TiAl alloy and the titanium alloy in the high-temperature environment can be met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of aeroengines, and in particular to an alloy coating and a preparation method and application thereof. Background Art

[0002] High thrust-to-weight ratio is an important indicator of aircraft engines, which involves two aspects: increasing the temperature of the combustion chamber and reducing the weight of the engine. Currently, nickel-based high-temperature alloys are the most widely used materials in aircraft engines, with good high-temperature mechanical properties. The service temperature limit of nickel-based high-temperature alloys is 1100°C, which is close to 80-90% of its melting point. It will be a great challenge to further increase the service temperature of nickel-based high-temperature alloys. In addition, the density of nickel-based high-temperature alloys is large (8.9g / cm 3 ), which restricts the weight reduction of aircraft engines.

[0003] TiAl alloy has low density (3.9-4.1g / cm 3 ), high yield strength, good creep resistance and other advantages, are gradually replacing traditional nickel-based high-temperature alloys to achieve lightweight and improved thrust-to-weight ratio of aircraft engines. However, some properties of TiAl alloys still need to be improved, especially the poor oxidation resistance above 800°C, which seriously limits its application. Under high temperature conditions, a mixed loose oxide layer of TiO2+Al2O3 will form on the surface of TiAl alloy instead of a single dense Al2O3 oxide layer, which is also the main reason for its insufficient oxidation resistance under high temperature conditions. Protective coatings have attracted widespread attention due to their economic, effective and non-changing advantages of the original composition and properties of the substrate. When the anti-oxidation coating prepared on the alloy surface is used in aircraft engines with harsh service environments, it is not only required that the coating has a high bonding strength with the alloy, but also that it should have good interface stability.

[0004] The current anti-oxidation coatings mainly include MCrAlY (M = Ni and / or Co), TiAlSiN and TiAlYN coatings, etc. Among them, MCrAlY coating is a mature anti-oxidation coating material with good service performance on nickel-based high-temperature alloys. However, the large difference in chemical composition between MCrAlY coating and TiAl alloy will lead to serious element interdiffusion between the two at high temperatures, rapid loss of Ni elements in the coating, the generation of a large number of Kirkendall holes, and the formation of hard and brittle Ni2 (Ti, Al) phase and Ni2 (Ti, Al)2 phase at the interface, thereby weakening the bonding force between the film and the substrate and reducing the mechanical properties of the alloy. In addition, with the extension of oxidation time, the internal stress generated by the deposition growth process and the thermal expansion coefficient of the coating (16×10 -6 K -1 -20×10 -6 K -1 ) and the thermal expansion coefficient of TiAl alloy (11×10-6 K -1 -13×10 -6 K -1 ) becomes increasingly different, which gradually deteriorates the interface stability of the system and eventually leads to coating peeling or failure.

[0005] Therefore, how to improve the interface compatibility between the antioxidant coating and TiAl alloy is the key to obtaining high-performance antioxidant coating materials. Summary of the invention

[0006] To solve the above problems, the present invention aims to provide an alloy coating and a preparation method and application thereof. The coating is an anti-oxidation coating on the surface of the alloy, which has the characteristics of high melting point and good chemical compatibility with TiAl alloy. The coating has high density and no obvious interdiffusion with TiAl alloy at high temperature. The appropriate amount of Al / Cr elements in the coating ensures that it has the ability to generate a continuous and dense Al2O3 phase, which can effectively improve the oxidation resistance of the alloy. In addition, the coating has a high bonding strength with the substrate, which can meet the use requirements of alloy substrates such as TiAl alloys in high temperature environments.

[0007] In order to achieve one of the above objects, a method for preparing the above alloy coating is provided, the method comprising the following steps:

[0008] TiAlCrNbRe alloy was used as target and TiAlCrNbRe anti-oxidation coating was prepared on the surface of alloy substrate by multi-arc ion plating.

[0009] Preferably, the multi-arc ion plating deposition adopts a current of 50-100A, a bias voltage of -300-0V, a temperature of 50-300°C, a working gas pressure of 0.8-2.0Pa, an argon gas flow rate of 100-200sccm, and a target-substrate distance of 50-100mm.

[0010] Preferably, the method further comprises: heat treating the coating sample after deposition; the heat treatment atmosphere is argon or vacuum; the heat treatment temperature is 800-1100° C., and the heat treatment time is 2-10 h.

[0011] Preferably, the method further comprises: performing sandblasting pretreatment on the TiAl alloy before the multi-arc ion plating deposition, wherein the sandblasting pressure is 0.1-0.6 MPa and the surface roughness of the TiAl alloy is 0.3-0.7 μm.

[0012] Preferably, the chemical components of the coating include Ti: 15-35at.%, Al: 35-55at.%, Cr: 15-35at.%, Nb: 1-10at.%, rare earth element Re≤3at.%; wherein the rare earth element Re is at least one of Ce, Gd, Yb, Lu, Y and Hf, and the sum of the atomic percentages of Ti, Al, Cr, Nb and Re is 100%.

[0013] The anti-oxidation coating provided by the present invention has a similar chemical composition to the TiAl alloy, ensuring good chemical compatibility between the coating and the alloy. The appropriate amount of Al in the coating enables the coating to generate a continuous and dense α-Al2O3 oxide layer. The introduction of Cr promotes the formation of a Laves phase with stronger anti-oxidation ability, and further promotes the formation of the Al2O3 oxide layer on the surface. The chemical composition of the anti-oxidation coating also includes a small amount of Nb and some rare earth elements. By adding an appropriate amount of Nb, Ti can be replaced. 4+ The vacancies in the coating form a Nb-rich solid solution phase, which improves the oxidation resistance of the coating. However, if the Nb element is excessive, it will hinder the formation of Al2O3. Wherein, the rare earth element Re includes at least one of Ce, Gd, Yb, Lu, Y and Hf, and the content is less than 3at.%. This appropriate content and type of rare earth element can pin the Al2O3 oxide layer on the surface of the coating and improve the anti-stripping ability of the oxide layer. However, excessive rare earth elements will aggravate the internal oxidation of the coating.

[0014] The second object of the present invention is to provide an alloy coating prepared according to the above preparation method. The present invention adopts the following technical solution:

[0015] An alloy coating, preferably, the coating has a thickness of 10-100 μm.

[0016] Furthermore, the thickness of the coating is 20-50 μm, so that the coating has good oxidation resistance and low interface stress.

[0017] Preferably, the thermal expansion coefficient of the coating in the temperature range from room temperature to 1000°C is 10.0×10 -6 K -1 17.0×10 -6 K -1 .

[0018] Furthermore, the thermal expansion coefficient of the coating in the temperature range from room temperature to 1000°C is 11.0×10 -6 K -1 -15.0×10 -6 K -1 .

[0019] Since the thermal expansion coefficient of TiAl alloy at room temperature -1000℃ is usually 9.0×10 -6 K -1 -14.0×10 -6 K -1 The thermal expansion coefficients of the above-mentioned anti-oxidation coating and the TiAl alloy are close, the stress generated under the influence of heat is small, the interface bonding of the coating is good, and it is not easy to fall off.

[0020] Furthermore, the phases formed by the anti-oxidation coating include γ-TiAl phase, Ti(Al,Cr)2Laves phase, AlCr2 phase and β-Cr phase.

[0021] The third object of the present invention is to provide an application of the above alloy coating, characterized in that the coating is used to form an anti-oxidation protection by bonding with the TiAl alloy or titanium alloy substrate. Specifically, after the TiAlCrNbRe anti-oxidation coating is oxidized at a high temperature of 900-1000°C for 20-500h, a dense oxide layer rich in α-Al2O3 phase is formed on the surface of the TiAl alloy or titanium alloy substrate.

[0022] Beneficial effects:

[0023] 1) The appropriate amount of Al / Cr elements in the coating of the present invention ensures that it has the ability to generate a continuous and dense Al2O3 phase, and the addition of an appropriate amount of Nb element can replace Ti 4+ The vacancies in the coating form a Nb-rich solid solution phase, which improves the oxidation resistance of the coating. An appropriate amount of rare earth elements can pin the Al2O3 oxide layer on the surface of the coating and improve the oxide layer's ability to resist spalling, thereby effectively improving the oxidation resistance of the alloy.

[0024] 2) The alloy coating of the present invention has the characteristics of high melting point and good chemical compatibility with alloy substrates such as TiAl alloys and titanium alloys, and can effectively reduce the mutual diffusion between the coating and the alloy.

[0025] 3) The coating prepared by the multi-arc ion plating method of the present invention has uniform thickness and high density, and there is no obvious interdiffusion between the TiAl alloy and the titanium alloy even at high temperature. In addition, the coating of the present invention has high bonding strength with the substrate, which can meet the use requirements of TiAl alloy and titanium alloy in high temperature environment. Thereby ensuring that when the anti-oxidation coating is applied to the alloy surface, not only the coating has high bonding strength with the alloy, but also has good interface stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] The present invention is further described below in conjunction with the accompanying drawings.

[0027] Figure 1It is a comparison diagram of thermal expansion coefficient curves of TiAl alloy, titanium alloy, TiAlCrNbRe coating of the present invention, and MCrAlY (M=Ni and / or Co) coating.

[0028] Figure 2 It is a schematic diagram of the structure of the anti-oxidation coating prepared on the TiAl alloy according to the present invention.

[0029] Figure 3a and Figure 3b They are respectively the surface micromorphology image and the cross-sectional micromorphology image of the TiAl alloy / anti-oxidation coating after heat treatment in Example 1 of the present invention.

[0030] Figure 4a and Figure 4b They are respectively an oxidation weight gain curve of the TiAl alloy / anti-oxidation coating of Example 1 of the present invention oxidized at 1000°C for 300 hours and an oxidation weight gain curve of the TiAl alloy oxidized at 1000°C for 50 hours.

[0031] Figure 5a and Figure 5b They are respectively the surface micromorphology and cross-sectional micromorphology of the TiAl alloy / anti-oxidation coating of Example 1 of the present invention after isothermal oxidation at 1000° C. for 300 hours.

[0032] Figure 6a and Figure 6b They are respectively the surface micromorphology and cross-sectional micromorphology of the TiAl alloy / anti-oxidation coating of Example 1 of the present invention after cyclic oxidation at 1000° C. for 200 h.

[0033] Figure 7a and Figure 7b They are respectively TiAl alloys prepared by plasma spraying in Comparative Example 2

[0034] Cross-sectional morphology of the / TiAlCrNbRe anti-oxidation coating and cross-sectional microscopic morphology after isothermal oxidation at 1000℃ for 300h.

[0035] Figure 8a and Figure 8b They are surface micromorphology and cross-sectional micromorphology of the TiAl alloy / anti-oxidation coating prepared by multi-arc ion plating with different process parameters after heat treatment in comparative example 3.

[0036] Figure 9a and Figure 9b They are respectively the surface micromorphology and cross-sectional micromorphology of the titanium alloy / anti-oxidation coating of Example 2 of the present invention after constant temperature oxidation at 800° C. for 300 hours.

[0037] Fig.10a and Fig.10bThey are respectively the surface micromorphology and cross-sectional micromorphology of the TiAl alloy / TiAlCrNbRe anti-oxidation coating after heat treatment in Example 3 of the present invention.

[0038] Fig.11a and Fig.11b They are respectively the surface micromorphology and cross-sectional micromorphology of the TiAl alloy / TiAlCrNbRe anti-oxidation coating after heat treatment in Example 4 of the present invention. DETAILED DESCRIPTION

[0039] The present invention is further explained in detail below in conjunction with the drawings and description of specific embodiments.

[0040] According to a preferred embodiment of the present invention, a method for preparing an alloy coating comprises the following steps:

[0041] TiAlCrNbRe alloy was used as target and TiAlCrNbRe anti-oxidation coating was prepared on the surface of alloy substrate by multi-arc ion plating.

[0042] The process parameters used for the multi-arc ion plating deposition are: current 50-100A, bias voltage -300-0V, temperature 50-300°C, working pressure 0.8-2.0Pa, argon flow rate 100-200sccm, target-substrate distance 50-100mm. If the parameters of multi-arc ion plating exceed the range, it will cause obvious defects to the coating. This process parameter range enables the coating to obtain a better thickness range and densification effect on the alloy substrate.

[0043] As a preferred embodiment, the method further comprises: heat treating the coating sample after deposition; the heat treatment atmosphere is argon or vacuum; the heat treatment temperature is 800-1100°C, and the heat treatment time is 2-20h. Specifically, the coating sample after multi-arc ion plating deposition can be placed in a vacuum atmosphere furnace for vacuum heat treatment to make the coating more uniform and dense.

[0044] The method may further include: performing sandblasting pretreatment on the alloy substrate, such as TiAl alloy or titanium alloy, before the multi-arc ion plating deposition, wherein the sandblasting pressure is 0.1-0.6 MPa, and the surface roughness of the alloy substrate TiAl after sandblasting is 0.3-0.7 μm.

[0045] Compared with traditional magnetron sputtering, plasma spraying and other technologies applied to TiAl alloy surfaces, the method used in the present invention has the characteristics of simple process, uniform and dense coating thickness, adjustable thickness range, good repeatability, high deposition efficiency and good winding performance.

[0046] In addition, the coating prepared by the method of this embodiment has high density and good bonding strength with the TiAl alloy substrate, which can lay a foundation for the application of anti-oxidation coatings in the field of aviation engines.

[0047] According to another preferred embodiment of the present invention, an alloy coating is prepared by the above-mentioned preparation method, wherein the coating includes Ti: 15-35at.%, Al: 35-55at.%, Cr: 15-35at.%, Nb: 1-10at.%, and rare earth element Re≤3at.%; wherein the rare earth element Re is at least one of Ce, Gd, Yb, Lu, Y and Hf, and the sum of the atomic percentages of Ti, Al, Cr, Nb and Re is 100%.

[0048] According to the coating provided in this embodiment, the TiAlCrNbRe layer is used as an anti-oxidation coating on the surface of an alloy substrate such as a TiAl alloy or a titanium alloy. In a high temperature environment, continuous and dense Al2O3 can be quickly generated, effectively isolating the alloy from contact with air and preventing the alloy from oxidizing. At the same time, since the coating has good chemical compatibility with the TiAl alloy and a close thermal expansion coefficient, the mutual diffusion between the coating and the alloy is effectively reduced, thereby enhancing the bonding strength of the interface and avoiding the occurrence of internal oxidation, and significantly improving the high-temperature oxidation resistance of the TiAl alloy.

[0049] Through research, it is found that the mechanism of the coating's good high-temperature oxidation resistance is that the phase composition of the TiAlCrNbRe coating after high-temperature oxidation mainly includes γ-TiAl phase, Ti(Al,Cr)2Laves phase and a small amount of β-Cr phase and AlCr2 phase. Among them, the Laves phase has a relatively high Al and Cr content and a high oxygen solubility, and has the ability to generate a continuous and dense Al2O3 oxide layer at high temperatures. At the same time, an appropriate amount of Nb element can replace Ti 4+ The vacancies in the coating form a Nb-rich solid solution phase, which improves the oxidation resistance of the coating; the γ-TiAl phase has the same structure as the alloy matrix, which makes the coating and the matrix more compatible; the β-Cr phase and the AlCr2 phase, as the initial oxidation products, can provide more Cr elements to combine with Ti and Al elements to generate Laves phases with better oxidation resistance. In addition, the appropriate amount of rare earth elements can pin the Al2O3 oxide layer on the coating surface and improve the anti-stripping ability of the oxide layer, thereby significantly improving the high-temperature oxidation resistance of the TiAl alloy.

[0050] As a preferred embodiment, the thickness of the coating is 10-100 μm. More preferably, the thickness of the coating is 20-50 μm. If the coating is too thick, on the one hand, due to the higher requirements of the application end scenario for lightweight and high-performance alloy materials, problems such as uneven coating thickness and poor adhesion are prone to occur, and the uniform and dense effect cannot be achieved. The internal oxidation phenomenon is serious during the service process, resulting in a decrease in the bonding strength of the coating; and, for some parts with smaller size requirements, when they are assembled and applied, there will be a problem of tolerance mismatch during assembly and it is difficult to apply; on the other hand, the difference in thermal expansion coefficient between the over-thick coating and the alloy will become larger, resulting in greater residual stress inside the coating, and eventually peeling and failure. If the coating is too thin, it is easy to oxidize the entire coating, which is not conducive to protecting the substrate. The present invention combines the method of preparing the coating by adopting a multi-arc ion plating deposition method, and the preparation method will be further described below, so that it can achieve a better dense effect in a relatively thin thickness range, so that the coating has good oxidation resistance and low interface stress.

[0051] like Figure 1 As shown in FIG. 1 , it is a comparison of thermal expansion coefficient curves of TiAl alloy, titanium alloy, TiAlCrNbRe coating of the present invention, and MCrAlY (M=Ni and / or Co) coating. It can be seen that the thermal expansion coefficient of the anti-oxidation coating of the present invention in the temperature range from room temperature to 1000°C is 10.0×10 -6 K -1 -17.0×10 -6 K -1 More preferably, by adjusting the chemical composition, the thermal expansion coefficient of the anti-oxidation coating in the temperature range from room temperature to 1000°C is 11.0×10 -6 K -1 -15.0×10 -6 K -1 Since the thermal expansion coefficient of TiAl alloy at room temperature -1000℃ is usually 9.0×10 -6 K -1 -14.0×10 -6 K -1 Compared with the existing MCrAlY (M = Ni and / or Co), the thermal expansion coefficient of the above-mentioned anti-oxidation coating is close to that of the TiAl alloy, the stress generated under the influence of heat is small, the interface bonding of the coating is good, and it is not easy to fall off.

[0052] The alloy coating provided by the present invention can be used to bond with a TiAl alloy or titanium alloy substrate to form an anti-oxidation protection for the alloy substrate, which can expand the application of the alloy substrate in the field of aeroengines. Specifically, after the TiAlCrNbRe anti-oxidation coating is oxidized at a high temperature of 900-1000°C for 20-500h, the coating will form a dense oxide layer rich in α-Al2O3 phase on the surface of the TiAl alloy or titanium alloy substrate, thereby achieving high-temperature oxidation resistance. The structure of the obtained coating on an alloy substrate such as TiAl is as follows: Figure 2 shown.

[0053] The following examples are further given to illustrate the present invention in detail. The specific process parameters and the like in the following examples are only examples within a suitable range, that is, those skilled in the art can make selections within a suitable range according to the description herein, and are not limited to the specific values ​​in the following examples.

[0054] Example 1

[0055] The alloy coating was prepared as follows:

[0056] Step 1: sandblasting the surface of the TiAl alloy at a sandblasting pressure of 0.4 MPa until the surface roughness is 0.5±0.1 μm, and ultrasonic cleaning to obtain a surface pretreated alloy;

[0057] Step 2: Design the chemical composition of the coating to be Ti: 28at.%, Al: 45at.%, Cr: 20at.%, Nb: 5at.%, Y: 2at.%, prepare the corresponding target raw materials, and use multi-arc ion plating technology to prepare the anti-oxidation coating of this component on the pretreated TiAl alloy surface. The process parameters of multi-arc ion plating deposition are shown in Table 1;

[0058] Table 1. Process parameters of multi-arc ion plating anti-oxidation coating

[0059] bias -100V Air pressure 1.5Pa Current 70A Argon flow rate 150sccm temperature 150℃ Target-substrate distance 70mm

[0060] Step 3: The TiAl alloy sample with the anti-oxidation coating is heat treated at 1000° C. for 2 hours in a vacuum atmosphere furnace to obtain a final coating on the alloy surface.

[0061] The surface micromorphology and cross-sectional micromorphology of the TiAl alloy / TiAlCrNbRe anti-oxidation coating after heat treatment in this embodiment are shown in Figures 1 and 2. Figure 3a and Figure 3b The TiAlCrNbRe anti-oxidation coating is dense, with small surface roughness, no large-diameter flying spots or molten droplets, and the coating thickness is uniform, about 35μm, well bonded with the alloy, and only tiny holes exist in the coating.

[0062] Performance test 1:

[0063] The oxidation weight gain value of the anti-oxidation coating is calculated by the weight gain method under high temperature and constant temperature conditions. The specific method is: when the temperature of the tube furnace rises to 1000°C, three parallel samples are placed in a dry crucible and placed in the constant temperature zone of 1000°C in the tube furnace, and weighed every 50 hours until 300 hours. The oxidation weight gain curve of the TiAl alloy / TiAlCrNbRe anti-oxidation coating prepared in this embodiment oxidized at 1000°C for 300 hours is shown in the figure below: Figure 4a The oxidation weight gain curve of TiAl alloy oxidized at 1000℃ for 50h is shown in Figure 4b The coating has a weight gain rate of less than 0.1 g / m after oxidation for 300 h. 2 h (reaching full oxidation resistance level); while the weight gain rate of the uncoated TiAl alloy after oxidation for 50 h is greater than 4 g / m 2 h (belonging to the weak oxidation resistance level), and the surface oxides began to fall off and form repeatedly, and subsequent weighing was no longer possible. It can be seen that the coating effectively reduces the oxidation weight gain rate of the TiAl alloy and improves the oxidation resistance of the TiAl alloy.

[0064] Performance test 2:

[0065] The anti-oxidation performance of the anti-oxidation coating was tested by high-temperature isothermal oxidation experiment. The specific method is: when the temperature of the tube furnace rises to 1000°C, three parallel samples are placed in the 1000°C isothermal zone of the tube furnace and kept warm for 300 hours. After the time is reached, the samples are cooled with the furnace and the cooled samples are cut, inlaid and polished. The surface micromorphology and cross-sectional micromorphology of the TiAl alloy / TiAlCrNbRe anti-oxidation coating prepared in this embodiment after isothermal oxidation for 300 hours are shown as follows: Figure 5a and Figure 5b As shown. After the sample was oxidized at 1000°C for 300 hours in an atmospheric environment, the surface oxide film was composed of a complete and dense Al2O3 oxide layer, and the coating was well bonded to the alloy without peeling, and the small holes in the coating were closed. In addition, there was no obvious interdiffusion between the coating and the TiAl alloy, indicating that the coating had good high-temperature stability. It can be seen that the TiAlCrNbRe coating prepared by multi-arc ion plating effectively improved the high-temperature oxidation resistance of the TiAl alloy.

[0066] Performance test three:

[0067] The TiAl alloy / TiAlCrNbRe coating was subjected to a more demanding high-temperature cyclic oxidation (anti-cyclic oxidation performance) test. The specific method is: when the temperature of the tube furnace rises to 1000°C, three parallel samples are placed in the constant temperature zone of the tube furnace at 1000°C and kept warm for 1 hour, then taken out and placed in the air for 10 minutes. This is one oxidation cycle. Repeat this process until the total insulation time reaches 200 hours. The cooled samples are cut, inlaid and polished. The surface micromorphology and cross-sectional micromorphology after 200 hours of oxidation test are shown as follows: Figure 6a and Figure 6b As shown in the figure, it can be found that the oxidation layer on the surface of the anti-oxidation coating is complete and dense, and the thickness is small, which indicates that the oxidation rate of the coating is low and the anti-oxidation performance is good. In addition, the coating does not peel off, which indicates that the coating and the alloy are well bonded.

[0068] Comparative Example 1

[0069] This comparative example is carried out with reference to Example 1, and the only difference from Example 1 is that the commercial NiCrAlY material is selected for the preparation of the anti-oxidation coating, and its chemical composition is Ni: 67at.%, Cr: 22at.%, Al: 10at.% and Y: 1.0at.%. The multi-arc ion plating deposition process parameters are shown in Table 2.

[0070] Table 2. Process parameters of multi-arc ion plating anti-oxidation coating

[0071] bias -100V Air pressure 1.5Pa Current 70A Argon flow rate 150sccm temperature 150℃ Target-substrate distance 70mm

[0072] The rest are the same as in Example 1 and will not be described again.

[0073] In the TiAl alloy / NiCrAlY coating prepared in this example, the NiCrAlY coating is about 35μm thick, the coating is uniform and dense, and it combines well with the TiAl alloy. There is serious interdiffusion between the NiCrAlY coating and the alloy, and the thickness of the interdiffusion zone is greater than 30μm. Moreover, the interdiffusion leads to the formation of Ni2TiAl phase and Ni(Ti,Al)2 phase with obvious hard and brittle characteristics at the interface between the coating and the alloy, which seriously damages the high-temperature mechanical properties of the TiAl alloy. In addition, the interdiffusion causes the elements of the coating to quickly flow into the alloy, and a large number of Kirkendall holes are generated inside the coating, causing it to fail quickly. Therefore, the traditional NiCrAlY coating has poor high-temperature stability on the surface of the TiAl alloy, and the high-temperature oxidation resistance life of the coating is insufficient.

[0074] Comparative Example 2

[0075] A TiCrAlNbRe anti-oxidation coating with the same chemical composition as in Example 1 was prepared on the surface of the TiAl alloy by vacuum plasma spraying, and an anti-oxidation test was performed after the same heat treatment. The vacuum plasma spraying process parameters are shown in Table 3.

[0076] Table 3. Vacuum plasma TiAlCrNbRe anti-oxidation spraying process parameters

[0077]

[0078] The cross-sectional microstructure of the TiAl alloy / TiCrAlNbRe coating sample prepared by conventional vacuum plasma spraying technology after heat treatment is shown in the figure below. Figure 7a The coating thickness is about 100 μm, and there are defects such as cracks and holes in the coating and at the interface between the coating and the substrate. The cross-sectional morphology of the TiAl alloy / anti-oxidation coating prepared by the vacuum plasma spraying technology after constant temperature oxidation at 1000℃ for 300h is shown in Figure 7b As shown. It can be seen that due to the large number of defects at the coating and the interface after heat treatment, oxygen penetrates into the coating during the oxidation process, resulting in serious internal oxidation. Furthermore, a large amount of Al2O3 is generated inside the coating and at the interface between the coating and the alloy, which aggravates and deteriorates the bonding strength between the coating and the alloy. Therefore, the anti-oxidation coating prepared on the surface of the TiAl alloy by the traditional preparation method has problems such as uneven coating thickness, poor adhesion, and many internal defects due to its large thickness, and cannot achieve a uniform and dense effect. During service, the internal oxidation phenomenon is serious, resulting in a decrease in the bonding strength of the coating. In addition, the TiAl alloy / anti-oxidation coating prepared by this technology is relatively thick, and when it is used in the assembly of some parts with smaller size requirements, there will be a problem of tolerance mismatch during assembly.

[0079] Comparative Example 3

[0080] This comparative example is carried out with reference to Example 1, and the only difference from Example 1 is that the multi-arc ion plating deposition process parameters are different, see Table 4.

[0081] Table 4. Process parameters of multi-arc ion plating anti-oxidation coating

[0082] bias 0V Air pressure 2.0Pa Current 150A Argon flow rate 150sccm temperature 150℃ Target-substrate distance 70mm

[0083] The surface and cross-sectional micromorphology of the TiAl alloy / TiCrAlNbRe coating samples prepared by multi-arc ion plating technology with different parameters after heat treatment are shown in the figure below. Figure 8a and Figure 8bAs shown. Since the current in the process parameters is large and no bias is applied, the surface roughness of the prepared coating is large, there are large flying points or particles, there are many defects such as cracks and holes inside the coating, and the coating is not uniform and dense enough, causing oxygen to penetrate into the coating during the oxidation process and causing serious internal oxidation. Furthermore, a large amount of Al2O3 is generated inside the coating, at the interface between the coating and the alloy, and inside the substrate, which aggravates and deteriorates the bonding strength between the coating and the alloy. Therefore, the use of inappropriate process parameters to prepare an anti-oxidation coating on the surface of TiAl alloy cannot achieve uniform and dense coating, and serious internal oxidation will occur during high-temperature service, resulting in a decrease in the bonding strength of the coating or even peeling.

[0084] Example 2

[0085] This embodiment is exactly the same as embodiment 1, the only difference being that the prepared coating is combined with a titanium alloy instead of a titanium-aluminum alloy.

[0086] Performance test 1:

[0087] The weight gain value of the oxidation-resistant coating was calculated by the weight gain method under high temperature and constant temperature conditions. The specific method is: when the temperature of the tube furnace rises to 800°C, three parallel samples are placed in a dry crucible and placed in the constant temperature zone of the tube furnace at 800°C, and weighed every 50 hours until 300 hours. The weight gain rate of the coating after oxidation for 300 hours is still less than 0.1g / m 2 h (reaching full oxidation resistance level); while the weight gain rate of titanium alloy without coating after oxidation for 50h is greater than 5g / m 2 h (belonging to the weak oxidation resistance level), and the surface oxides began to fall off and form repeatedly, and subsequent weighing was no longer possible. It can be seen that the coating effectively reduces the oxidation weight gain rate of the TiAl alloy and improves the oxidation resistance of the titanium alloy.

[0088] Performance test 2:

[0089] The anti-oxidation performance of the anti-oxidation coating was tested by high-temperature isothermal oxidation experiment. The specific method is: when the temperature of the tube furnace rises to 800°C, three parallel samples are placed in the constant temperature zone of the tube furnace at 1000°C and kept warm for 300 hours. After the time is reached, the samples are cooled with the furnace and the cooled samples are cut, inlaid and polished. The surface micromorphology and cross-sectional micromorphology of the titanium alloy / TiAlCrNbRe anti-oxidation coating prepared in this embodiment after isothermal oxidation for 300 hours are shown as follows: Figure 9a and Figure 9bAs shown. After the sample was oxidized at 800°C for 300 hours in an atmospheric environment, the surface oxide film was composed of a complete and dense Al2O3 oxide layer, and the coating was well bonded to the alloy without peeling, and the small holes in the coating were closed. In addition, there was no obvious interdiffusion between the coating and the TiAl alloy, indicating that the coating had good high-temperature stability. It can be seen that the TiAlCrNbRe coating prepared by multi-arc ion plating effectively improves the high-temperature oxidation resistance of titanium alloy.

[0090] Example 3

[0091] This embodiment is basically the same as embodiment 1, the only difference being the chemical composition of the coating:

[0092] Ti: 15at.%, Al: 55at.%, Cr: 25at.%, Nb: 3at.%, Ce: 2at.%.

[0093] The surface micromorphology and cross-sectional micromorphology of the TiAl alloy / TiAlCrNbRe anti-oxidation coating after heat treatment in this embodiment are shown in Figures 1 and 2. Fig.10a and Fig.10b The TiAlCrNbRe anti-oxidation coating is dense, with small surface roughness, no large-diameter flying spots or molten droplets, and the coating thickness is uniform, about 40μm, well bonded to the alloy, and only tiny holes exist in the coating.

[0094] Example 4

[0095] This embodiment is basically the same as embodiment 1, the only difference being the chemical composition of the coating:

[0096] Ti: 35at.%, Al: 37at.%, Cr: 17at.%, Nb: 10at.%, Y: 1at.%.

[0097] The surface micromorphology and cross-sectional micromorphology of the TiAl alloy / TiAlCrNbRe anti-oxidation coating after heat treatment in this embodiment are shown in Figures 1 and 2. Fig.11a and Fig.11b The TiAlCrNbRe anti-oxidation coating is dense, with small surface roughness, no large-diameter flying spots or molten droplets, and the coating thickness is uniform, about 20μm, well bonded to the alloy, and only tiny holes exist in the coating.

[0098] The above embodiments are only used to further illustrate the technical solution of the present invention in detail and cannot be understood as limiting the protection scope of the present invention. Some non-essential improvements and adjustments made by technicians in this field based on the above content of the present invention belong to the protection scope of the present invention.

Claims

1. A method for preparing an alloy coating, It is characterized in that The method comprises the following steps: TiAlCrNbRe alloy was used as target and TiAlCrNbRe anti-oxidation coating was prepared on the surface of alloy substrate by multi-arc ion plating.

2. The method according to claim 1, Features: The multi-arc ion plating deposition adopts a current of 50-100A, a bias voltage of -300-0V, a temperature of 50-300°C, a working gas pressure of 0.8-2.0Pa, an argon gas flow rate of 100-200sccm, and a target-substrate distance of 50-100mm.

3. The method according to claim 1 or 2, It is characterized in that The method also includes: heat treating the coating sample after deposition; the heat treatment atmosphere is argon or vacuum; and the heat treatment temperature is controlled to be 800-1100° C. and the heat treatment time is 2-20 hours.

4. The method according to claim 1 or 2, It is characterized in that The method may also include: performing sandblasting pretreatment on the alloy substrate before multi-arc ion plating deposition; controlling the pressure of the sandblasting to be 0.1-0.6 MPa, and sandblasting until the surface roughness of the alloy substrate TiAl is 0.3-0.7 μm.

5. The method according to claim 1 or 2, It is characterized in that The chemical components of the coating include Ti: 15-35at.%, Al: 35-55at.%, Cr: 15-35at.%, Nb: 1-10at.%, and rare earth element Re≤3at.%; wherein the rare earth element Re is at least one of Ce, Gd, Yb, Lu, Y and Hf, and the sum of the atomic percentages of Ti, Al, Cr, Nb and Re is 100%.

6. An alloy coating, prepared according to the method according to any one of claims 1 to 5, It is characterized in that The coating has a thickness of 10-100 μm.

7. The alloy coating according to claim 6, It is characterized in that The coating has a thickness of 20-50 μm.

8. The alloy coating according to claim 7, It is characterized in that The thermal expansion coefficient of the coating in the temperature range from room temperature to 1000°C is 10.0×10 -6 K -1 -17.0×10 -6 K -1 .

9. The alloy coating according to claim 7, It is characterized in that The coating phases include γ-TiAl phase, Ti(Al,Cr) 2 Laves phase, AlCr 2 phase and β-Cr phase.

10. Use of the alloy coating according to any one of claims 6 to 9, It is characterized in that The coating is used for surface bonding with a TiAl alloy or titanium alloy substrate to form anti-oxidation protection.

Citation Information

Cited By

  • Laves phase-containing layer based on control rod guide tube Cr coating and preparation method of Laves phase-containing layer

    CN119710556A