Coating for high-temperature brazing tool, tool knife and device
By forming a mixed metal powder and skeleton material coating with a thickness of 10-50μm on the surface of the diamond brazing layer, the problem of low cracks and bonding force of diamond tools in the high-temperature brazing process is solved, and the bending strength of the tool is significantly improved. The wear ratio extends the service life.
Patent Information
- Application Number
- CN202410959792.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-29
AI Technical Summary
In high-temperature brazing process, diamond tools are prone to cracks and low bonding force, which affects their grinding performance and service life.
The coating for high-temperature brazing tools formed on the surface of the diamond brazing layer is adopted. The raw material composition of the coating includes mixed metal powder and skeleton materials, such as YG8, WC, Cr3C2, TiC, TiAlN, DLC, etc., through chemical vapor deposition or physical Vapor deposition technology forms a thin coating with a thickness of 10-50 μm to improve the strength of the brazing layer and prevent cracks.
It effectively improves the bending strength and wear ratio of the diamond brazing layer, significantly extends the service life of the tool, and maintains grinding performance under high temperature conditions of 800℃, avoiding cracks and desoldering and crushing.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of brazing, and in particular relates to a coating, a tool knife and a device for a high-temperature brazing tool. Background Art
[0002] Diamond grinding tools are an important type of cutting equipment. The diamond brazed grinding layer structure they provide has good processability and structural stability. The diamond abrasives in it are not easy to peel off, and have good grinding performance and service life for high-hardness materials. For example, diamond needles are used clinically for tooth preparation, pit and fissure shaping, hard fillings and dental metal material cutting, etc.; diamond needles are used in denture processing factories mainly for denture grinding. Whether it is a needle used clinically or a needle used in a denture processing factory, its appearance and structure are varied. Each dentist or technician uses needles of different specifications and shapes for tooth preparation or grinding according to their own operating habits and usage methods, and finally realizes tooth preparation and denture grinding. At present, in the high-temperature brazing process, diamond is prone to structural defects such as cracks at high temperatures such as above 800°C, while in the high-temperature brazing process, the long-term grinding performance and service life of the tool will be affected due to defects such as low bonding force.
[0003] Therefore, in view of the above technical problems, it is necessary to provide a coating, a tool knife and a device for high-temperature brazing tools.
[0004] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention
[0005] The object of the present invention is to provide a coating, a tool knife and a device for high-temperature brazing tools.
[0006] In order to achieve the above object, a technical solution provided by a specific embodiment of the present invention is as follows:
[0007] A coating for high-temperature brazing tools is formed on the surface of a diamond brazing layer. The diamond brazing layer is a grinding layer formed by fixing diamond abrasives to the tool surface through a brazing process using a brazing material. The raw material composition of the coating includes, by weight: 80-95% mixed metal powder and the remainder skeleton material, wherein the skeleton material is selected from: YG8, WC, Cr3C2, TiC, TiCN, TiAlN, DLC, TaC; the mixed metal powder is selected from several of Cu, Sn, Cr, Ti, Fe, Ni, and Ag.
[0008] In one or more embodiments of the present invention, the coating has a thickness of 10-50 μm.
[0009] In one or more embodiments of the present invention, when the diamonds in the grinding layer are uniformly distributed particles of the same size, the coating is a thin layer with uniform thickness, and the thickness is 10-20 μm.
[0010] In one or more embodiments of the present invention, when the diamond particles in the grinding layer are different particles of the same size, the coating is a thin layer with a uniform thickness of 30-50 μm.
[0011] In high-temperature brazing structures, in order to improve the wetting effect on defective structures, a longer coating film-forming time is used to form a thicker coating film-forming effect, thereby effectively improving the defect problems caused by the brazing operation.
[0012] In one or more embodiments of the present invention, the mixed metal powder is a mixture of Cu, Sn, Cr, Ti, Fe, Ni, and Ag.
[0013] In one or more embodiments of the present invention, the mass ratio of Cu, Sn, Cr, Ti, Fe, Ni and Ag in the mixed metal powder is: 4:2:1:0.7:1.2:0.6:0.5.
[0014] In one or more embodiments of the present invention, the skeleton material is a mixture of at least one of YG8 and TiC and DLC.
[0015] In one or more embodiments of the present invention, the proportion of DLC in the skeleton material is 5-10%.
[0016] In one or more embodiments of the present invention, a tool knife includes a tool body having a diamond coating and a coating for a high-temperature brazing tool as described above formed at least on the surface of a blade portion of the tool body.
[0017] In one or more embodiments of the present invention, a grinding device includes a main machine and a tool knife as described above connected to a driving device of the main machine.
[0018] Compared with the prior art, the coating, tool knife and device for high-temperature brazing tools of the present invention effectively overcome the problems of product performance and life caused by damage to diamond in high-temperature brazing technology, such as cracks caused by high temperature leading to reduced diamond grinding performance and reduced service life, thereby providing a thin film coating formed on the surface of the brazing layer to effectively protect the grinding structure of the diamond brazing layer. DETAILED DESCRIPTION
[0019] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0020] The coating for high-temperature brazing tools of the present invention can be formed on the surface of the diamond brazing layer by existing technologies such as chemical vapor deposition and physical vapor deposition. The diamond brazing layer is a grinding layer formed by fixing diamond abrasives to the tool surface through a brazing process using a brazing material to overcome the defects of the diamond brazing layer formed by high-temperature brazing, such as low bonding force and low strength.
[0021] The present invention includes but is not limited to the following embodiments, wherein the raw materials of the brazing filler metal for diamond brazing include, by mass fraction, 45 parts of copper, 9 parts of silver, 30 parts of zinc, 2.8 parts of nickel, 0.5 parts of graphene powder material with a particle size of 80 microns, 0.2 parts of magnesium carbonate, and 0.95 parts of rosin. The brazing filler metal is uniformly dispersed by a process such as sufficient mixing and melting. The number of brazing layers formed on the tool by brazing is 3, and the thickness of a single layer is 150 microns.
[0022] According to the relevant national standards (GB5319-85, Determination of transverse fracture strength of sintered metal materials), the size of the segment specimen is determined, the span spacing of the three-point bending fixture is 25mm, and the load drop speed is 1mm / min. A 30×6×10 rectangular grinding wheel segment is prepared, and the average value of the three specimens is used as the final test result to obtain the bending strength value.
[0023] Grinding test
[0024] Maximum circumferential speed of tool sample: 25m / s
[0025] Grinding fluid: 5% water-based emulsion, flow rate 90L / min
[0026] Grinding machine: creep feed surface grinder, model MMD7125
[0027] Grinding method: Plunge grinding
[0028] Table feed speed: 0.3m / min
[0029] Grinding test results: Using sample workpiece to grind Al 2 O 3 Ceramic grinding experiment, Al 2 O 3 The ceramics were subjected to a continuous grinding test, with the test endpoint being when the exposed part of the abrasive had lost 60% of its height.
[0030] Example 1
[0031] The coating for high-temperature brazing tools in this embodiment has a functional raw material composition including, by weight: 80% mixed metal powder and the balance skeleton material, wherein the skeleton material is YG8; the mixed metal powder is a mixture of Cu, Sn, and Cr in a mass ratio of 1:1:1 (the powder particles are all 150 mesh, the same below).
[0032] On the dental bur brazed with a grinding layer at a brazing temperature of 800°C, when the diamonds in the grinding layer are evenly distributed particles of the same size of about 0.5 mm, the coating on the surface of the grinding layer is a thin layer of uniform thickness, with a thickness of 10 μm: the three-point bending strength value of the sample block is 157 MPa, and there is no desoldering or breakage of the abrasive on the surface of the bur after the grinding experiment, and there are no cracks under microscopic observation, and the wear ratio is greater than 300.
[0033] On the cutting blade with a grinding layer brazed at a brazing temperature of 800°C, when the diamonds in the grinding layer are evenly distributed particles of the same size of about 0.5 mm, the coating on the surface of the grinding layer is a thin layer with uniform thickness of 10 μm: the three-point bending strength value of the sample block is 153 MPa, and there is no desoldering or breakage of the abrasive on the surface of the turning needle after the grinding experiment, and there are no cracks under microscopic observation, and the wear ratio is greater than 300.
[0034] On the dental bur brazed with a grinding layer at a brazing temperature of 800°C, when the diamond in the grinding layer is distributed in particles of about 1 mm in the highest linear speed area, about 0.5 mm in the lowest linear speed area, and 0.6 mm in the rest, the coating on the surface of the grinding layer is a thin layer with uniform thickness of 30 μm: the three-point bending strength value of the sample block is 155 MPa, and there is no desoldering or breakage of the abrasive on the surface of the bur after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 300.
[0035] On the cutting blade brazed with a grinding layer at a brazing temperature of 800°C, when the diamond in the grinding layer is distributed in the area of highest linear speed with a particle size of about 1 mm, in the area of lowest linear speed with a particle size of about 0.5 mm, and the rest with a particle size of 0.8 mm, the coating on the surface of the grinding layer is a thin layer with a uniform thickness of 30 μm: the three-point bending strength value of the sample block is 152 MPa, and there is no desoldering or breakage of the abrasive on the surface of the turning needle after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 350.
[0036] Example 2
[0037] The coating for high-temperature brazing tools in this embodiment has a functional raw material composition comprising, by weight: 88% mixed metal powder and the remainder skeleton material, wherein the skeleton material is selected from: Cr3C2; the mixed metal powder is selected from a mixture of Cu, Sn, Fe, and Ni in a mass ratio of 1:0.2:0.2:0.5.
[0038] On the dental bur brazed with a grinding layer at a brazing temperature of 800°C, when the diamonds in the grinding layer are evenly distributed particles of the same size of about 0.5 mm, the coating on the surface of the grinding layer is a thin layer of uniform thickness with a thickness of 10 μm: the three-point bending strength value of the sample block is 151 MPa, and there is no desoldering or breakage of the abrasive on the surface of the bur after the grinding experiment, and there are no cracks under microscopic observation, and the wear ratio is greater than 350.
[0039] On the cutting blade with a grinding layer brazed at a brazing temperature of 800°C, when the diamonds in the grinding layer are evenly distributed particles of the same size of about 0.5 mm, the coating on the surface of the grinding layer is a thin layer with uniform thickness of 10 μm: the three-point bending strength value of the sample block is 150 MPa, and there is no desoldering or breakage of the abrasive on the surface of the turning needle after the grinding experiment, and there are no cracks under microscopic observation, and the wear ratio is greater than 350.
[0040] On the dental bur brazed with a grinding layer at a brazing temperature of 800°C, when the diamond in the grinding layer is distributed in the area of highest linear speed with a particle size of about 1 mm, in the area of lowest linear speed with a particle size of about 0.5 mm, and the rest with a particle size of 0.6 mm, the coating on the surface of the grinding layer is a thin layer with a uniform thickness of 30 μm: the three-point bending strength value of the sample block is 153 MPa, and there is no desoldering or breakage of the abrasive on the surface of the bur after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 350.
[0041] On the cutting blade brazed with a grinding layer at a brazing temperature of 800°C, when the diamond in the grinding layer is distributed in the area of highest linear speed with a particle size of about 1 mm, in the area of lowest linear speed with a particle size of about 0.5 mm, and the rest with a particle size of 0.8 mm, the coating on the surface of the grinding layer is a thin layer with a uniform thickness of 30 μm: the three-point bending strength value of the sample block is 154 MPa, and there is no desoldering or breakage of the abrasive on the surface of the turning needle after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 350.
[0042] Example 3
[0043] The coating for high-temperature brazing tools in this embodiment has a functional raw material composition comprising, by weight: 95% mixed metal powder and the remainder skeleton material, wherein the skeleton material is selected from: TaC; the mixed metal powder is selected from a mixture of Ti, Fe, Ni, and Ag in a mass ratio of 1:3:1:0.5.
[0044] On the dental needle brazed with a grinding layer at a brazing temperature of 800℃, when the diamonds in the grinding layer are evenly distributed particles of the same size of about 0.5mm, the coating on the surface of the grinding layer is a thin layer with uniform thickness of 10μm: the three-point bending strength value of the sample block is 162MPa, and there is no desoldering or breakage of the abrasive on the surface of the needle after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 400.
[0045] On the cutting blade with a grinding layer brazed at a brazing temperature of 800°C, when the diamonds in the grinding layer are evenly distributed particles of the same size of about 0.5 mm, the coating on the surface of the grinding layer is a thin layer with uniform thickness of 10 μm: the three-point bending strength value of the sample block is 168 MPa, and there is no desoldering or breakage of the abrasive on the surface of the turning needle after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 400.
[0046] On the dental bur brazed with a grinding layer at a brazing temperature of 800°C, when the diamond in the grinding layer is distributed in the area of highest linear speed with a particle size of about 1 mm, in the area of lowest linear speed with a particle size of about 0.5 mm, and the rest with a particle size of 0.6 mm, the coating on the surface of the grinding layer is a thin layer with a uniform thickness of 30 μm: the three-point bending strength value of the sample block is 165 MPa, and there is no desoldering or breakage of the abrasive on the surface of the bur after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 400.
[0047] On the cutting blade brazed with a grinding layer at a brazing temperature of 800°C, when the diamond in the grinding layer is distributed in the area of highest linear speed with a particle size of about 1 mm, in the area of lowest linear speed with a particle size of about 0.5 mm, and the rest with a particle size of 0.8 mm, the coating on the surface of the grinding layer is a thin layer with a uniform thickness of 30 μm: the three-point bending strength value of the sample block is 160 MPa, and there is no desoldering or breakage of the abrasive on the surface of the turning needle after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 400.
[0048] Example 4
[0049] The only difference between this embodiment and embodiment 1 is that the mixed metal powder is a mixture of Cu, Sn, Cr, Ti, Fe, Ni, and Ag, and the mass ratio thereof is 4:2:1:0.7:1.2:0.6:0.5.
[0050] On the dental bur brazed with a grinding layer at a brazing temperature of 800°C, when the diamonds in the grinding layer are evenly distributed particles of the same size of about 0.5 mm, the coating on the surface of the grinding layer is a thin layer of uniform thickness, with a thickness of 10 μm: the three-point bending strength value of the sample block is 189 MPa, and there is no desoldering or breakage of the abrasive on the surface of the bur after the grinding experiment, and there are no cracks under microscopic observation, and the wear ratio is greater than 550.
[0051] On the cutting blade with a grinding layer brazed at a brazing temperature of 800°C, when the diamonds in the grinding layer are evenly distributed particles of the same size of about 0.5 mm, the coating on the surface of the grinding layer is a thin layer with uniform thickness of 10 μm: the three-point bending strength value of the sample block is 185 MPa, and there is no desoldering or breakage of the abrasive on the surface of the turning needle after the grinding experiment, and there are no cracks under microscopic observation, and the wear ratio is greater than 550.
[0052] On the dental bur brazed with a grinding layer at a brazing temperature of 800°C, when the diamond in the grinding layer is distributed in the area of highest linear speed with a particle size of about 1 mm, in the area of lowest linear speed with a particle size of about 0.5 mm, and the rest with a particle size of 0.6 mm, the coating on the surface of the grinding layer is a thin layer with a uniform thickness of 30 μm: the three-point bending strength value of the sample block is 187 MPa, and there is no desoldering or breakage of the abrasive on the surface of the bur after the grinding experiment, and there are no cracks under microscopic observation, and the wear ratio is greater than 550.
[0053] On the cutting blade brazed with a grinding layer at a brazing temperature of 800°C, when the diamond in the grinding layer is distributed in the area of highest linear speed with a particle size of about 1 mm, in the area of lowest linear speed with a particle size of about 0.5 mm, and the rest with a particle size of 0.8 mm, the coating on the surface of the grinding layer is a thin layer with a uniform thickness of 30 μm: the three-point bending strength value of the sample block is 188 MPa, and there is no desoldering or breakage of the abrasive on the surface of the turning needle after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 550.
[0054] Example 5
[0055] The only difference between this embodiment and embodiment 4 is that the framework material is a mixture of TiC and DLC in a mass ratio of 1:1.
[0056] On the dental bur brazed with a grinding layer at a brazing temperature of 800°C, when the diamonds in the grinding layer are evenly distributed particles of the same size of about 0.5 mm, the coating on the surface of the grinding layer is a thin layer with uniform thickness of 10 μm: the three-point bending strength value of the sample block is 186 MPa, and there is no desoldering or breakage of the abrasive on the surface of the bur after the grinding experiment, and there are no cracks under microscopic observation, and the wear ratio is greater than 550.
[0057] On the cutting blade with a grinding layer brazed at a brazing temperature of 800°C, when the diamonds in the grinding layer are evenly distributed particles of the same size of about 0.5 mm, the coating on the surface of the grinding layer is a thin layer with uniform thickness of 10 μm: the three-point bending strength value of the sample block is 178 MPa, and there is no desoldering or breakage of the abrasive on the surface of the turning needle after the grinding experiment, and there are no cracks under microscopic observation, and the wear ratio is greater than 550.
[0058] On the dental bur brazed with a grinding layer at a brazing temperature of 800°C, when the diamond in the grinding layer is distributed in the area of highest linear speed with a particle size of about 1 mm, in the area of lowest linear speed with a particle size of about 0.5 mm, and the rest with a particle size of 0.6 mm, the coating on the surface of the grinding layer is a thin layer with a uniform thickness of 30 μm: the three-point bending strength value of the sample block is 182 MPa, and there is no desoldering or breakage of the abrasive on the surface of the bur after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 550.
[0059] On the cutting blade brazed with a grinding layer at a brazing temperature of 800°C, when the diamond in the grinding layer is distributed in the area of highest linear speed with a particle size of about 1 mm, in the area of lowest linear speed with a particle size of about 0.5 mm, and the rest with a particle size of 0.8 mm, the coating on the surface of the grinding layer is a thin layer with a uniform thickness of 30 μm: the three-point bending strength value of the sample block is 187 MPa, and there is no desoldering or breakage of the abrasive on the surface of the turning needle after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 550.
[0060] Example 6
[0061] The only difference between this embodiment and embodiment 4 is that the framework material is a mixture of YG8 and DLC in a mass ratio of 1:1.
[0062] On the dental bur brazed with a grinding layer at a brazing temperature of 800°C, when the diamonds in the grinding layer are evenly distributed particles of the same size of about 0.5 mm, the coating on the surface of the grinding layer is a thin layer of uniform thickness with a thickness of 10 μm: the three-point bending strength value of the sample block is 183 MPa, and there is no desoldering or breakage of the abrasive on the surface of the bur after the grinding experiment, and there are no cracks under microscopic observation, and the wear ratio is greater than 550.
[0063] On the cutting blade with a grinding layer brazed at a brazing temperature of 800°C, when the diamonds in the grinding layer are evenly distributed particles of the same size of about 0.5 mm, the coating on the surface of the grinding layer is a thin layer with uniform thickness of 10 μm: the three-point bending strength value of the sample block is 184 MPa, and there is no desoldering or breakage of the abrasive on the surface of the turning needle after the grinding experiment, and there are no cracks under microscopic observation, and the wear ratio is greater than 550.
[0064] On the dental bur brazed with a grinding layer at a brazing temperature of 800°C, when the diamond in the grinding layer is distributed in the area of highest linear speed with a particle size of about 1 mm, in the area of lowest linear speed with a particle size of about 0.5 mm, and the rest with a particle size of 0.6 mm, the coating on the surface of the grinding layer is a thin layer with a uniform thickness of 30 μm: the three-point bending strength value of the sample block is 182 MPa, and there is no desoldering or breakage of the abrasive on the surface of the bur after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 550.
[0065] On the cutting blade brazed with a grinding layer at a brazing temperature of 800°C, when the diamond in the grinding layer is distributed in the area of highest linear speed with a particle size of about 1 mm, in the area of lowest linear speed with a particle size of about 0.5 mm, and the rest with a particle size of 0.8 mm, the coating on the surface of the grinding layer is a thin layer with a uniform thickness of 30 μm: the three-point bending strength value of the sample block is 185 MPa, and there is no desoldering or breakage of the abrasive on the surface of the turning needle after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 550.
[0066] Example 7
[0067] The only difference between this embodiment and embodiment 4 is that the framework material is a mixture of YG8, TiC, and DLC in a mass ratio of 54:38:8.
[0068] On the dental bur brazed with a grinding layer at a brazing temperature of 800°C, when the diamonds in the grinding layer are evenly distributed particles of the same size of about 0.5 mm, the coating on the surface of the grinding layer is a thin layer with uniform thickness of 10 μm: the three-point bending strength value of the sample block is 197 MPa, and there is no desoldering or breakage of the abrasive on the surface of the bur after the grinding experiment, and there are no cracks under microscopic observation, and the wear ratio is greater than 550.
[0069] On the cutting blade with a grinding layer brazed at a brazing temperature of 800°C, when the diamonds in the grinding layer are evenly distributed particles of the same size of about 0.5 mm, the coating on the surface of the grinding layer is a thin layer with uniform thickness of 10 μm: the three-point bending strength value of the sample block is 195 MPa, and there is no desoldering or breakage of the abrasive on the surface of the turning needle after the grinding experiment, and there are no cracks under microscopic observation, and the wear ratio is greater than 550.
[0070] On the dental bur brazed with a grinding layer at a brazing temperature of 800°C, when the diamond in the grinding layer is distributed in the area of highest linear speed with a particle size of about 1 mm, in the area of lowest linear speed with a particle size of about 0.5 mm, and the rest with a particle size of 0.6 mm, the coating on the surface of the grinding layer is a thin layer with a uniform thickness of 30 μm: the three-point bending strength value of the sample block is 195 MPa, and there is no desoldering or breakage of the abrasive on the surface of the bur after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 550.
[0071] On the cutting blade brazed with a grinding layer at a brazing temperature of 800°C, when the diamond in the grinding layer is distributed in the area of highest linear speed with a particle size of about 1 mm, in the area of lowest linear speed with a particle size of about 0.5 mm, and the rest with a particle size of 0.8 mm, the coating on the surface of the grinding layer is a thin layer with a uniform thickness of 30 μm: the three-point bending strength value of the sample block is 193 MPa, and there is no desoldering or breakage of the abrasive on the surface of the turning needle after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 550.
[0072] Example 8
[0073] The only difference between this embodiment and embodiment 4 is that the framework material is a mixture of YG8, TiC, and DLC in a mass ratio of 15:4:1.
[0074] On the dental bur brazed with a grinding layer at a brazing temperature of 800°C, when the diamonds in the grinding layer are evenly distributed particles of the same size of about 0.5 mm, the coating on the surface of the grinding layer is a thin layer with uniform thickness of 10 μm: the three-point bending strength value of the sample block is 192 MPa, and there is no desoldering or breakage of the abrasive on the surface of the bur after the grinding experiment, and there are no cracks under microscopic observation, and the wear ratio is greater than 550.
[0075] On the cutting blade with a grinding layer brazed at a brazing temperature of 800°C, when the diamonds in the grinding layer are evenly distributed particles of the same size of about 0.5 mm, the coating on the surface of the grinding layer is a thin layer of uniform thickness, with a thickness of 10 μm: the three-point bending strength value of the sample block is 193 MPa, and there is no desoldering or breakage of the abrasive on the surface of the turning needle after the grinding experiment, and there are no cracks under microscopic observation, and the wear ratio is greater than 550.
[0076] On the dental bur brazed with a grinding layer at a brazing temperature of 800°C, when the diamond in the grinding layer is distributed in the area of highest linear speed with a particle size of about 1 mm, in the area of lowest linear speed with a particle size of about 0.5 mm, and the rest with a particle size of 0.6 mm, the coating on the surface of the grinding layer is a thin layer with a uniform thickness of 30 μm: the three-point bending strength value of the sample block is 196 MPa, and there is no desoldering or breakage of the abrasive on the surface of the bur after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 550.
[0077] On the cutting blade brazed with a grinding layer at a brazing temperature of 800°C, when the diamond in the grinding layer is distributed in the area of highest linear speed with a particle size of about 1 mm, in the area of lowest linear speed with a particle size of about 0.5 mm, and the rest with a particle size of 0.8 mm, the coating on the surface of the grinding layer is a thin layer with a uniform thickness of 30 μm: the three-point bending strength value of the sample block is 195 MPa, and there is no desoldering or breakage of the abrasive on the surface of the turning needle after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 550.
[0078] Example 9
[0079] The only difference between this embodiment and embodiment 4 is that the framework material is a mixture of YG8, TiC, and DLC in a mass ratio of 5:4:1.
[0080] On the dental bur brazed with a grinding layer at a brazing temperature of 800°C, when the diamonds in the grinding layer are evenly distributed particles of the same size of about 0.5 mm, the coating on the surface of the grinding layer is a thin layer of uniform thickness with a thickness of 10 μm: the three-point bending strength value of the sample block is 205 MPa, and there is no desoldering or breakage of the abrasive on the surface of the bur after the grinding experiment, and there are no cracks under microscopic observation, and the wear ratio is greater than 550.
[0081] On the cutting blade with a grinding layer brazed at a brazing temperature of 800°C, when the diamonds in the grinding layer are evenly distributed particles of the same size of about 0.5 mm, the coating on the surface of the grinding layer is a thin layer with uniform thickness of 10 μm: the three-point bending strength value of the sample block is 207 MPa, and there is no desoldering or breakage of the abrasive on the surface of the turning needle after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 550.
[0082] On the dental bur brazed with a grinding layer at a brazing temperature of 800°C, when the diamond in the grinding layer is distributed in the area of highest linear speed with a particle size of about 1 mm, in the area of lowest linear speed with a particle size of about 0.5 mm, and the rest with a particle size of 0.6 mm, the coating on the surface of the grinding layer is a thin layer with uniform thickness of 30 μm: the three-point bending strength value of the sample block is 207 MPa, and there is no desoldering or breakage of the abrasive on the surface of the bur after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 550.
[0083] On the cutting blade brazed with a grinding layer at a brazing temperature of 800°C, when the diamond in the grinding layer is distributed in the area of highest linear speed with a particle size of about 1 mm, in the area of lowest linear speed with a particle size of about 0.5 mm, and the rest with a particle size of 0.8 mm, the coating on the surface of the grinding layer is a thin layer with a uniform thickness of 30 μm: the three-point bending strength value of the sample block is 209 MPa, and there is no desoldering or breakage of the abrasive on the surface of the turning needle after the grinding experiment, and there is no crack under microscopic observation, and the wear ratio is greater than 550.
[0084] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.
[0085] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A coating for high-temperature brazing tools, which is formed on the surface of a diamond brazing layer, wherein the diamond brazing layer is a grinding layer formed by fixing diamond abrasives to the tool surface through a brazing process using a brazing material, characterized in that: The raw material composition of the coating The invention comprises: wt%: 80-95% of mixed metal powder and the balance of skeleton material, wherein the skeleton material is selected from: YG8, WC, Cr3C2, TiC, TiCN, TiAlN, DLC, TaC; the mixed metal powder is selected from several of Cu, Sn, Cr, Ti, Fe, Ni and Ag.
2. The coating for high temperature brazing tools according to claim 1, characterized in that: The coating has a thickness of 10-100 μm.
3. The coating for high temperature brazing tools according to claim 2, characterized in that: When the diamonds in the grinding layer are uniformly distributed particles of the same size, the coating is a thin layer with uniform thickness, and the thickness is 10-20 μm.
4. The coating for high temperature brazing tools according to claim 2, characterized in that: When the diamonds in the grinding layer are particles of different sizes, the coating is a thin layer with uniform thickness, and the thickness is 30-50 μm.
5. The coating for high temperature brazing tools according to claim 1, characterized in that: The mixed metal powder is a mixture of Cu, Sn, Cr, Ti, Fe, Ni and Ag.
6. The coating for high temperature brazing tools according to claim 5, characterized in that: The mass ratio of Cu, Sn, Cr, Ti, Fe, Ni and Ag in the mixed metal powder is: 4:2:1:0.7:1.2:0.6:0.
5.
7. The coating for high temperature brazing tools according to claim 1, characterized in that: The framework material is a mixture of at least one of YG8 and TiC and DLC.
8. The coating for high temperature brazing tools according to claim 7, characterized in that: The DLC accounts for 5-10% in the skeleton material.
9. A tool knife comprising a tool body having a diamond coating and the coating for high temperature brazing tools according to any one of claims 1 to 8 formed at least on the surface layer of the blade of the tool body.
10. A grinding device comprising a main machine and the utility knife according to claim 9 connected to a driving device of the main machine.