Preparation method of single-crystal rod-like LiV3O8 positive electrode material with high oxygen vacancy content
Through the direct calcination method of lithium fluoride and vanadium pentoxide, single crystal rod-shaped LiV3O8 with high oxygen vacancy content was prepared, which solved the problems of complex process and low oxygen vacancy content in the prior art, and significantly improved the rate cycle performance of LiV3O8 and cycle life.
Patent Information
- Application Number
- CN202411162873.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-29
AI Technical Summary
The existing methods have complex processes for manufacturing oxygen vacancy defects, long time periods, large energy consumption and low oxygen vacancy content, and cannot fully utilize the electrochemical performance of LiV3O8, resulting in poor rate cycling performance and unexpected capacity attenuation.
Lithium fluoride and vanadium pentoxide were mixed with vanadium pentoxide and directly roasted to form single crystal rod-shaped LiV3O8 with high oxygen vacancy content. By controlling the molar ratio, atmosphere and temperature, efficient preparation of oxygen vacancy defects is achieved, and the structural stability and electron transport of LiV3O8 are improved. efficiency.
Significantly improve the rate cycle performance and cycle life of LiV3O8, maintain structural stability, and achieve high specific capacity and long cycle life performance.
Smart Images

Figure CN119041001A_ABST
Abstract
Description
Technical Field
[0001] The invention provides a method for preparing a single crystal rod-shaped LiV3O8 positive electrode material with a high oxygen vacancy content, belonging to the technical field of electrochemical materials. Background Art
[0002] The development of lithium-ion battery (LIB) cathode materials is a key factor in promoting battery performance. With the rapid development of portable electronic devices, power tools, electric vehicles and energy storage systems, the demand for high-performance lithium-ion batteries is increasing. However, LiCoO2, LiMn2O4, LiFePO4, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 The energy and power density of lithium-ion batteries based on cathode materials such as O2 are still unsatisfactory, and vanadium oxides have attracted widespread attention due to their high theoretical specific capacity. Vanadates (such as LiV3O8) are particularly noteworthy. Although LiV3O8 has a high specific capacity, its rate performance is still poor and its capacity is prone to unexpected attenuation.
[0003] It is reported that by creating oxygen vacancy (OV) defects, the intrinsic ion diffusion rate and high conductivity of the electrode material can be improved, and lithium ion diffusion can be promoted, charge transfer resistance can be reduced, and the capacity and cycle stability of LiV3O8 can be improved. At present, the main methods for obtaining OV in transition metal oxides are heat treatment annealing, plasma irradiation, reduction flame roasting, supercritical fluid processing, gas-solid interface reaction and mechanical grinding. Ji et al. (Electro chem. Soc., 2018, 165, A2880–A2888.) proved that under high pressure and supercritical CO2 treatment, OV can be obtained in Li 1.2 Mn 0.56 N i0.16 Co 0.08 O2 cathode material was successfully formed. Chen et al. (Alloys Compd, 2019, 803, 71–79.) reported that OV was uniformly distributed on LiNi under the interaction of plasma bombardment and mechanical milling. 0.5 Co 0.2 Mn 0.3 On the surface of O2-SnO2 positive electrode material. Song et al. (Mater. Interfaces, 2017, 9, 2875–2882.) reported the successful synthesis of oxygen-deficient LiV3O8 by hydrothermal reaction and subsequent heat treatment annealing in argon. The prepared LiV3O8 exhibited significant capacity characteristics and excellent lithium ion storage stability at different current densities. -1 After 200 cycles, the initial reversible capacity can still be maintained at more than 88%.
[0004] The above methods for producing oxygen vacancy (OV) defects are complex, time-consuming, energy-intensive, and require high equipment. However, the oxygen vacancy content of the electrode materials prepared is still low, and the excellent electrochemical performance of LiV3O8 cannot be fully utilized. Therefore, there are still great limitations on further improving the rate cycling performance of LiV3O8.
[0005] The present invention adopts a new process to directly prepare a single-crystal rod-shaped LiV3O8 powder with a high oxygen vacancy content in one step. The reaction process is simple, energy-saving and efficient to directly produce oxygen vacancy (OV) defects, and its content is as high as more than 10%, which can greatly improve the rate cycle performance of LiV3O8. The particle size of the single-crystal rod-shaped LiV3O8 prepared by the reaction is micron-sized, and the micron-sized size can improve the structural stability of LiV3O8, reduce the side reactions on the surface of LiV3O8, and improve the tap density. The single-crystal rod-shaped structure helps to improve the electron transmission and ion diffusion efficiency of lithium-ion positive electrode materials, because its one-dimensional morphology provides a more continuous conductive path and a shorter ion diffusion distance, thereby significantly improving the rate performance and cycle life of LiV3O8. Therefore, the new method of the present invention, which uses lithium fluoride and vanadium pentoxide to mix and then directly roast in one step to generate rod-shaped single-crystal LiV3O8 with a high oxygen vacancy content, is of great significance. Summary of the invention
[0006] The purpose of the present invention is to provide a method for preparing a single-crystal rod-shaped LiV3O8 positive electrode material with a high oxygen vacancy content. The method uses lithium fluoride and vanadium pentoxide as raw materials for reaction, and can prepare single-crystal rod-shaped LiV3O8 with a high oxygen vacancy content, wherein the oxygen vacancy defects can greatly improve the rate cycle performance of LiV3O8, the micron-level size can improve the structural stability of LiV3O8, reduce the side reactions on the surface of LiV3O8, and increase the tap density, and the single-crystal rod-shaped structure helps to improve the electron transmission and ion diffusion efficiency of lithium ion positive electrode materials. Thereby solving the problem of poor rate performance and unexpected capacity attenuation of LiV3O8.
[0007] A method for preparing a single-crystalline rod-shaped LiV3O8 positive electrode material with a high oxygen vacancy content, characterized in that:
[0008] Step 1: Using lithium fluoride powder as the lithium source of LiV3O8 and vanadium pentoxide powder as the vanadium source of LiV3O8;
[0009] Step 2: Mix and grind lithium fluoride and vanadium pentoxide in a certain molar ratio to obtain a mixed powder;
[0010] Step 3: In a certain atmosphere, keep the mixed powder at a certain temperature for a period of time and then cool it to room temperature to obtain a single crystal rod-shaped LiV3O8 material with a high oxygen vacancy content.
[0011] The certain molar ratio is 0.5-2.0:1.0.
[0012] The certain atmosphere is an oxidizing atmosphere, a reducing atmosphere or an inert atmosphere.
[0013] The certain temperature is 400-550°C.
[0014] The period of time is ≤4.0h.
[0015] Beneficial effects of the present invention: high oxygen vacancy content can effectively prevent the accidental dissolution of vanadium during the rate cycle of LiV3O8 and the surface side reaction of LiV3O8, maintain the structural stability of LiV3O8, and achieve high rate and long cycle life performance of LiV3O8 as a positive electrode material for lithium ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 This is the XRD pattern of the rod-shaped single crystal LiV3O8 with high oxygen vacancy content generated by the reaction.
[0017] Figure 2 This is the SEM image of the rod-shaped single crystal LiV3O8 with high oxygen vacancy content generated by the reaction.
[0018] Figure 3 This is the XPS graph of the rod-shaped single crystal LiV3O8 with high oxygen vacancy content generated by the reaction.
[0019] Figure 4 At a current density of 50 mA -1 Charge and discharge curves of rod-shaped single-crystalline LiV3O8 with high oxygen vacancy content.
[0020] Figure 5 This is the rate cycling diagram of rod-shaped single crystal LiV3O8 with high oxygen vacancy content at a current density of 2C. DETAILED DESCRIPTION
[0021] The present invention will be further described below in conjunction with specific implementation modes.
[0022] Example 1
[0023] The preparation method of the positive electrode material rod-shaped single crystal LiV3O8 with high oxygen vacancy content comprises the following steps:
[0024] The preparation method uses raw material lithium fluoride as a lithium source and raw material vanadium pentoxide as a vanadium source; lithium fluoride powder and vanadium pentoxide powder with a molar ratio of 1.0:1.0 are mixed and ground, and the mixed powder is heated to 550°C in an argon atmosphere and kept warm for 0.5h to generate a rod-shaped single crystal LiV3O8 with an oxygen vacancy content of 10.7% (see Figure 3 ). The prepared pure phase single crystal LiV3O8 (see Figure 1 ), the average diameter of the rods of LiV3O8 is 2.1um and the average length is 8.0um (see Figure 2 ).
[0025] Example 2
[0026] The preparation method of the positive electrode material rod-shaped single crystal LiV3O8 with high oxygen vacancy content comprises the following steps:
[0027] The preparation method uses raw material lithium fluoride as a lithium source and raw material vanadium pentoxide as a vanadium source; lithium fluoride powder and vanadium pentoxide powder with a molar ratio of 1.5:1.0 are mixed and ground, and the mixed powder is heated to 500°C in an air-oxidizing atmosphere and kept warm for 2.0 hours to generate rod-shaped single crystal LiV3O8 with an oxygen vacancy content of 14.5%.
[0028] Example 3
[0029] The preparation method of the positive electrode material rod-shaped single crystal LiV3O8 with high oxygen vacancy content comprises the following steps:
[0030] The preparation method uses raw material lithium fluoride as a lithium source and raw material vanadium pentoxide as a vanadium source; lithium fluoride powder and vanadium pentoxide powder with a molar ratio of 2.0:1.0 are mixed and ground, and the mixed powder is heated to 450°C in a hydrogen atmosphere and kept warm for 3.0 hours to generate rod-shaped single crystal LiV3O8 with an oxygen vacancy content of 11.2%.
[0031] Example 4
[0032] The preparation method of the positive electrode material rod-shaped single crystal LiV3O8 with high oxygen vacancy content comprises the following steps:
[0033] The preparation method uses raw material lithium fluoride as a lithium source and raw material vanadium pentoxide as a vanadium source; lithium fluoride powder and vanadium pentoxide powder with a molar ratio of 0.5:1.0 are mixed and ground, and the mixed powder is heated to 400°C in a nitrogen atmosphere and kept warm for 4.0 hours to generate rod-shaped single crystal LiV3O8 with an oxygen vacancy content of 12.1%.
[0034] Example 5
[0035] The preparation method of the positive electrode material rod-shaped single crystal LiV3O8 with high oxygen vacancy content comprises the following steps:
[0036] The preparation method uses raw material lithium fluoride as a lithium source and raw material vanadium pentoxide as a vanadium source; lithium fluoride powder and vanadium pentoxide powder with a molar ratio of 1.5:1.0 are mixed and ground, and the mixed powder is heated to 550°C in an oxygen atmosphere and kept warm for 0.1h to generate rod-shaped single crystal LiV3O8 with an oxygen vacancy content of 10.2%.
[0037] Electrochemical performance test
[0038] The test items of the present invention are as follows:
[0039] Preparation and performance test of button half-cell:
[0040] The preparation method of button half-cell is as follows: first, active positive electrode materials LiV3O8, PVDF and carbon black are mixed in a mass ratio of 8:1:1, and a proper amount of NMP is added and stirred to form battery slurry, and then the battery slurry is evenly coated on aluminum foil and placed in a 100°C oven for 12 hours. After drying, the positive electrode sheets are cut into round sheets of uniform size, and the loading amount of active substances on the sheets is 1-2 mg / cm 2 . The positive electrode sheet prepared above was placed in a vacuum glove box, and the metal lithium sheet was used as the negative electrode, and assembled into a button-type half-cell with the separator, electrolyte and other components. After the assembly was completed, the charge and discharge tests at different current densities of 1.5 to 4.0V were carried out on the LAND CT-2000A battery tester. The test environment conditions were a constant room temperature of 25°C, and the charge cut-off voltage and discharge cut-off voltage were 4.0V and 1.5V respectively. When the LiV3O8 prepared in Example 1 was charged at 50mAg -1 At a current density of 1.5 %, the discharge capacity is as high as 316 mAhg -1 (See Figure 4 ), which reflects the excellent high specific capacity and high energy density performance of the rod-shaped single crystal LiV3O8 with high oxygen vacancy content prepared by this method. When the LiV3O8 prepared in Example 1 is subjected to a high current density of 2C, the initial capacity is as high as 158.6 mAhg -1 After 500 cycles, the capacity retention rate reached 84.2% and the reversible capacity still reached 133.6 mAh g -1 (See Figure 5 ). This shows that the rod-shaped single crystal LiV3O8 with high oxygen vacancy content prepared by this method has excellent high rate and long cycle life performance.
Claims
1. A method for preparing a single-crystalline rod-shaped LiV3O8 positive electrode material with a high oxygen vacancy content, characterized in that: Step 1: Using lithium fluoride powder as the lithium source of LiV3O8 and vanadium pentoxide powder as the vanadium source of LiV3O8; Step 2: Mix and grind lithium fluoride and vanadium pentoxide in a certain molar ratio to obtain a mixed powder; Step 3: In a certain atmosphere, keep the mixed powder at a certain temperature for a period of time and then cool it to room temperature to obtain a single crystal rod-shaped LiV3O8 material with a high oxygen vacancy content.
2. The method for preparing a single-crystalline rod-shaped LiV3O8 positive electrode material with a high oxygen vacancy content according to claim 1, characterized in that: The certain molar ratio is 0.5-2.0:1.
0.
3. The method for preparing a single-crystalline rod-shaped LiV3O8 positive electrode material with a high oxygen vacancy content according to claim 1, characterized in that: The certain atmosphere is an oxidizing atmosphere, a reducing atmosphere or an inert atmosphere.
4. The method for preparing a single-crystalline rod-shaped LiV3O8 positive electrode material with a high oxygen vacancy content according to claim 1, characterized in that: The certain temperature is 400-550°C.
5. The method for preparing a single-crystalline rod-shaped LiV3O8 positive electrode material with a high oxygen vacancy content according to claim 1, characterized in that: The period of time is ≤4.0h.