Antibacterial material as well as preparation method and application thereof
A broad-spectrum antibacterial material was prepared by combining a mixture of casone, bronitol, butylcarbamate, with a heat stabilizer and a light stabilizer, which solved the single effect of existing antibacterial materials on mold and preparation technology. Complex problems achieve efficient killing and lasting effects of various molds, and show the advantages of safety and environmental protection in textiles.
Patent Information
- Application Number
- CN202411225309.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-29
AI Technical Summary
The existing antibacterial materials have a single effect on mold inhibition and killing, and the preparation process is complex and cannot be promoted on a large scale. The killing ability of various molds is limited, and the scope of use and durability are insufficient.
A mixture of casone, bromnol and iodopropynyl butycarbamate is used as anti-mold fungicide, and a heat stabilizer and light stabilizer are added to form a broad-spectrum antibacterial material through simple stirring and uniform preparation method. Suitable for textiles, etc.
This antibacterial material has extremely high killing ability to various molds, has a small amount of use, a wide range of application, a long-lasting effect, and is simple in preparation, safe and environmentally friendly, which can effectively prevent the growth of mold in textiles and provide anti-aging effects.
Smart Images

Figure BDA0005024314720000031 
Figure BDA0005024314720000032 
Figure BDA0005024314720000041
Abstract
Description
Technical Field
[0001] The invention relates to D06M13, and in particular to an antibacterial material and a preparation method and application thereof. Background Art
[0002] Antibacterial materials have an inhibitory and killing effect on microorganisms, so that the product maintains a good appearance and physical properties. Commonly used antibacterial agents include textile antibacterial agents, cosmetic antibacterial agents, papermaking antibacterial agents, leather antibacterial agents, and feed antibacterial agents, etc., with a wide variety. Patent document CN111134136A discloses an RO non-oxidative slime control and bactericide and its preparation method and application. The raw materials include, by mass percentage: 10-20% of kason, 5-10% of bronopol, 2-5% of sodium chloride, 10-20% of potassium chloride, and the rest is deionized water. The sum of the mass percentages of all raw materials is 100%. It can be used to clean and sterilize the reverse osmosis system, has good sterilization effect, can reduce the frequency and time of cleaning and sterilization, and improve the utilization rate and production efficiency of the reverse osmosis system. However, it has the disadvantage of only inhibiting and killing several specific molds and single antibacterial performance. Invention patent CN105076133B discloses a composite cationic mildew inhibitor, which can actively adsorb and kill surrounding negatively charged bacteria, fungi, etc. The drug-carrying layer and sustained-release layer of the mildew-proof card can play a dual sterilization role, can effectively sterilize in a larger space, and has a prolonged effective period, but has the problem of complex process and cannot be promoted on a large scale.
[0003] In view of the shortcomings of the prior art, the present application proposes an antibacterial material having extremely high killing ability against various molds, small dosage, wide application range, long-lasting efficacy, simple preparation process, convenient operation, safety and environmental protection, as well as its preparation method and application. Summary of the invention
[0004] In order to solve the above problems existing in the prior art, the present invention provides an antibacterial material and a preparation method and application thereof.
[0005] An antibacterial material, characterized in that the raw materials for preparation include, by weight:
[0006] 0.7-2.1 parts of antifungal agent
[0007] Heat stabilizer 0.05-0.18 parts
[0008] Solvent 90-110 parts
[0009] Light stabilizer 0.05-0.15 parts
[0010] As a preferred embodiment, the mildew-proofing and fungicide is selected from one or a mixture of bronopol, kasone, phenoxyethanol, and iodopropynyl butylcarbamate.
[0011] Preferably, the mildew and fungicide is a mixture of kason, bronopol and iodopropynyl butylcarbamate. More preferably, the weight ratio of kason, bronopol and iodopropynyl butylcarbamate is 2:1:3. As a preferred embodiment, the heat stabilizer is an inorganic heat stabilizer.
[0012] Preferably, the inorganic heat stabilizer is nitrate.
[0013] More preferably, the nitrate is sodium nitrate, and the weight portion is 0.08 parts.
[0014] As a preferred embodiment, the solvent is an inorganic solvent and / or an organic solvent.
[0015] Preferably, the inorganic solvent is water, and the organic solvent is selected from one or a combination of two or more of ethylene glycol, propylene glycol, polyethylene glycol, butylene glycol, polypropylene glycol, triethanolamine, pentaerythritol, mannitol, and triethylene glycol.
[0016] More preferably, the organic solvent selected in the present application is a mixture of propylene glycol and polyethylene glycol, with a weight ratio of 17:32.
[0017] As a preferred embodiment, the light stabilizer is a hindered amine light stabilizer.
[0018] In a previous patent application for a mildew-proof agent for textiles and a method for preparing the same, the applicant used kason and bronopol to quickly kill mildew on the surface and shallow layer of textiles, which was particularly suitable for cellulose textiles and leather products. However, the applicant unexpectedly discovered in a series of research and improvement experiments that when the weight ratio of kason, bronopol, and iodopropynyl butylcarbamate is 2:1:3, adding a light stabilizer thereto can greatly increase the duration of action and the bactericidal effect of the mildew-proof agent.
[0019] The present invention also provides a method for preparing the mildew-proofing and fungicide: adding the mildew-proofing and fungicide, a heat stabilizer and a light stabilizer into a solvent and stirring the mixture evenly.
[0020] The invention also provides an application of the mildew-proofing and fungicide: application in textiles.
[0021] Beneficial Effects
[0022] 1. Kasong has a good inhibitory effect on yeast, fungi, Gram-negative bacteria, algae, etc. Adding inorganic stabilizer sodium nitrate to it can increase the thermal stability of the solution.
[0023] 2. Nitro alcohol can effectively prevent and control a variety of plant pathogenic bacteria; iodopropynyl butylcarbamate can effectively kill molds, yeasts, algae and bacteria, and has special effects on fungi. The present invention uses kason, nitro alcohol and iodopropynyl butylcarbamate to compound, which has extremely high killing ability against various molds, small dosage, wide application range and long-lasting effect.
[0024] 3. The preparation process of the mildew inhibitor provided by the present invention is simple, convenient to operate, safe and environmentally friendly.
[0025] 4. Antifungal fungicides are non-irritating, non-corrosive and non-volatile, so they have little impact on the textile production and use environment.
[0026] 5. The mildew-proofing and fungicide provided by the present invention can be applied to textiles, and after adding a light stabilizer, it can have an anti-aging effect on the textiles. DETAILED DESCRIPTION
[0027] Example 1 An antibacterial material and its preparation method and application (I) is prepared from the following raw materials in parts by weight
[0028]
[0029] The chlorine ratio of the Kathon is 3.2, purchased from Guangzhou Nipantech Technology Co., Ltd.; the sodium nitrate is purchased from Jilin Rongxin Chemical Co., Ltd.; the solvent includes an organic solvent and water, and the organic solvent is a mixture of propylene glycol and polyethylene glycol, with a weight ratio of 17:32; the polyethylene glycol has a relative molecular mass of 400, purchased from Renda Chemical Co., Ltd.; the weight ratio of the organic solvent to water is 20:1; the hindered amine light stabilizer is purchased from Nantong Runfeng Petrochemical Co., Ltd.
[0030] (II) Preparation method
[0031] Add kason, bronopol, iodopropynyl butylcarbamate, sodium nitrate and hindered amine light stabilizer into the solvent and stir evenly.
[0032] Example 2 An antibacterial material and its preparation method and application (I) is prepared from the following raw materials in parts by weight
[0033]
[0034] The chlorine ratio of the Kathon is 3.2, purchased from Guangzhou Nipantech Technology Co., Ltd.; the sodium nitrate is purchased from Jilin Rongxin Chemical Co., Ltd.; the solvent includes an organic solvent and water, and the organic solvent is a mixture of propylene glycol and polyethylene glycol, with a weight ratio of 17:32; the polyethylene glycol has a relative molecular mass of 400, purchased from Renda Chemical Co., Ltd.; the weight ratio of the organic solvent to water is 20:1; the hindered amine light stabilizer is purchased from Nantong Runfeng Petrochemical Co., Ltd.
[0035] (II) Preparation method
[0036] Add kason, bronopol, iodopropynyl butylcarbamate, sodium nitrate and hindered amine light stabilizer into the solvent and stir evenly.
[0037] Example 3 An antibacterial material and its preparation method and application (I) is prepared from the following raw materials in parts by weight
[0038]
[0039] The chlorine ratio of the Kathon is 3.2, purchased from Guangzhou Nipantech Technology Co., Ltd.; the sodium nitrate is purchased from Jilin Rongxin Chemical Co., Ltd.; the solvent includes an organic solvent and water, and the organic solvent is a mixture of propylene glycol and polyethylene glycol, with a weight ratio of 17:32; the polyethylene glycol has a relative molecular mass of 400, purchased from Renda Chemical Co., Ltd.; the weight ratio of the organic solvent to water is 20:1; the hindered amine light stabilizer is purchased from Nantong Runfeng Petrochemical Co., Ltd.
[0040] (II) Preparation method
[0041] Add kason, bronopol, iodopropynyl butylcarbamate, sodium nitrate and hindered amine light stabilizer into the solvent and stir evenly.
[0042] Example 4 An antibacterial material and its preparation method and application (I) is prepared from the following raw materials in parts by weight
[0043]
[0044]
[0045] The chlorine ratio of the Kathon is 3.2, purchased from Guangzhou Nipantech Technology Co., Ltd.; the sodium nitrate is purchased from Jilin Rongxin Chemical Co., Ltd.; the solvent includes an organic solvent and water, and the organic solvent is a mixture of propylene glycol and polyethylene glycol, with a weight ratio of 17:32; the polyethylene glycol has a relative molecular mass of 400, purchased from Renda Chemical Co., Ltd.; the weight ratio of the organic solvent to water is 20:1; the hindered amine light stabilizer is purchased from Nantong Runfeng Petrochemical Co., Ltd.
[0046] (II) Preparation method
[0047] Add kason, bronopol, iodopropynyl butylcarbamate, sodium nitrate and hindered amine light stabilizer into the solvent and stir evenly.
[0048] Comparative Example 1 An antibacterial material and its preparation method and application (I) is prepared from the following raw materials in parts by weight
[0049]
[0050] The chlorine ratio of the Kathon is 3.2, purchased from Guangzhou Nipantech Technology Co., Ltd.; the sodium nitrate is purchased from Jilin Rongxin Chemical Co., Ltd.; the solvent includes an organic solvent and water, and the organic solvent is a mixture of propylene glycol and polyethylene glycol, with a weight ratio of 17:32; the polyethylene glycol has a relative molecular mass of 400, purchased from Renda Chemical Co., Ltd.; the weight ratio of the organic solvent to water is 20:1; the hindered amine light stabilizer is purchased from Nantong Runfeng Petrochemical Co., Ltd.
[0051] (II) Preparation method
[0052] Add kason, bronopol, iodopropynyl butylcarbamate, sodium nitrate and hindered amine light stabilizer into the solvent and stir evenly.
[0053] Comparative Example 2 An antibacterial material and its preparation method and application (I) is prepared from the following raw materials in parts by weight
[0054]
[0055] The chlorine ratio of the Kathon is 3.2, purchased from Guangzhou Nitrogen Technology Co., Ltd.; the sodium nitrate is purchased from Jilin Rongxin Chemical Co., Ltd.; the solvent includes an organic solvent and water, the organic solvent is a mixture of propylene glycol and polyethylene glycol, and the weight ratio is 17:32; the polyethylene glycol has a relative molecular mass of 400, purchased from Renda Chemical Co., Ltd.; the weight ratio of the organic solvent to water is 20:1.
[0056] (II) Preparation method
[0057] Add kason, bronopol, iodopropynyl butylcarbamate, sodium nitrate and hindered amine light stabilizer into the solvent and stir evenly.
[0058] Performance Testing
[0059] 1. Anti-mildew test
[0060] A 1200 mL cylindrical glass container was soaked with detergent, rinsed with clean water, wiped with 75% ethanol, and then placed on a clean bench for ultraviolet disinfection. 200 mL of sterile water was poured in, and a cotton cloth sprayed with 2 mL of a 1*108 / mL mold spore suspension was hung in the cylindrical glass container, and 1 mL of the mildew inhibitor obtained in Examples 1 to 8 was sprayed. The cylindrical glass container was sealed and placed in a constant temperature and humidity incubator at 28° C. and 95% humidity for 60 days, and the growth of mycelium in the cotton cloth was recorded: no mycelium growth was seen on the surface of the sample, which was recorded as level 0; no mycelium growth was seen on the surface of the sample, but the mycelium growth area did not exceed one-third of the total area, which was recorded as level 1; mycelium growth was seen on the surface of the sample, and the mycelium growth area exceeded one-third of the total area, but did not exceed two-thirds of the total area, which was recorded as level 2; mycelium growth was seen on the surface of the sample, and the mycelium growth area exceeded two-thirds of the total area, which was recorded as level 3.
[0061] Table 1: Mildew resistance test grade evaluation table
[0062]
[0063]
Claims
1. An antibacterial material, It is characterized in that The raw materials for preparation are calculated by weight and include: 0.7-2.1 parts of mildew and fungicide; Heat stabilizer 0.05-0.18 parts; 90-110 parts of solvent; Light stabilizer 0.05-0.15 parts.
2. The antibacterial material according to claim 1, Features: The mildew-proofing and fungicide is selected from one or a mixture of bronopol, kasone, phenoxyethanol, and iodopropynyl butylcarbamate.
3. The antibacterial material according to claim 1, Features: The heat stabilizer is an inorganic heat stabilizer.
4. The antibacterial material according to claim 1, Features: The solvent is an inorganic solvent and / or an organic solvent.
5. The antibacterial material according to claim 3, Features: The inorganic heat stabilizer is nitrate.
6. The antibacterial material according to claim 1, Features: The light stabilizer is a hindered amine light stabilizer.
7. The antibacterial material according to claim 4, Features: The inorganic solvent is water.
8. The antibacterial material according to claim 4, Features: The organic solvent is selected from one or a combination of two or more of ethylene glycol, glycerol, polyethylene glycol, butylene glycol, polyglycerol, triethanolamine, pentaerythritol, mannitol, and triethylene glycol.
9. A method for preparing the antibacterial material according to any one of claims 1 to 8, Features: Add the mildew preventer, heat stabilizer and light stabilizer into the solvent and stir evenly.
10. An antibacterial material according to any one of claims 1 to 8 applied to textiles.