Method for dynamically regulating and controlling solidification of ecological bottom mud based on clay mineral composition

By using the curing activity of industrial solid waste to stimulate the index and clay mineral activity during the curing process, a green process is designed to solve the problems of high cement curing costs and environmental pollution, and an efficient and economical curing effect of the bottom sludge is achieved. It also promotes the resource utilization of industrial solid waste.

CN119041389AActive Publication Date: 2024-11-29CHINA THREE GORGES UNIV

Patent Information

Application Number
CN202411016654.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-29
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

The prior art has problems such as high cement use cost, large greenhouse gas emissions, long curing time and large energy consumption in the process of curing the bottom sludge, and the failure to effectively utilize industrial solid waste, resulting in environmental pollution and waste of resources.

Method used

By using the curing activity excitation index and aluminum, calcium and silicon rate control models based on the industrial solid waste, combined with the clay mineral activity in the base sludge, a curing agent that can significantly cure the base sludge is designed, and a simple green process is used to reduce energy Consumption and improve curing effect.

Benefits of technology

It has achieved efficient curing of the base sludge, significantly improved the compressive strength after curing, reduced the amount of cement, promoted the resource utilization of industrial solid waste, complied with the goal of green and low-carbon development, and the process is simple and economical.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119041389A_ABST
    Figure CN119041389A_ABST
Patent Text Reader

Abstract

River and lake bottom mud is soft soil with high water content and organic matters, and has the bad engineering characteristics of high compressibility, large porosity, low strength and the like. Usually, after a tedding and drying method is adopted for pretreatment, cement, lime and other curing materials are added to serve as road filler, time, labor and money are wasted, and the environment is polluted. The invention relates to a method for preparing a bottom mud curing composite base material by taking pretreated bottom mud with high water content as road filler and reasonably utilizing a potential curing activity excitation concept in industrial solid waste. According to the method, a framework for designing components of the bottom mud curing agent from the aspects of gelling and dense strength is established from the perspective of'treating waste with waste '. Under the condition that the activity of clay minerals in bottom mud is considered, bulk industrial solid wastes such as yellow phosphorus slag, blast furnace slag and carbide slag are introduced into preparation of the ecological curing agent, the doping amount of a curing material is dynamically regulated and controlled according to active components in the clay minerals and the solid wastes, the activity of the clay minerals and the solid wastes is stimulated to the maximum extent, and the curing effect is improved. The method can be applied to design evaluation of solid waste solidified bottom mud.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of foundation treatment in transportation engineering and civil engineering, and specifically relates to a dynamic control method for ecological sediment solidification based on clay mineral composition. Background Art

[0002] Cement-lime mixture for solidifying sediment is a commonly used reinforcement technology at home and abroad, in which cement is the main solidifying material of this method. In the process of solidifying sediment, cement can react chemically to form a solid granular material, thereby achieving the solidification of sediment and effectively solving the problem of sediment treatment. Cement solidified sediment can reduce the volume of sediment, and the solidified sediment can be used as a building material, such as roadbed filler, etc., thereby reducing the treatment cost. The solidified sediment can reduce the emission of harmful substances in the sediment and avoid harm to the environment. However, appropriate cement and lime need to be added during the solidification process. When the amount of sediment is large, the cost will be relatively high; cement will produce a large amount of greenhouse gases such as carbon dioxide during the solidification process, which greatly affects the environment; cement solidified sediment takes a certain amount of time to solidify, which will increase the time cost. Although the technology of using cement to solidify sediment is simple, a large amount of greenhouse gases will be released during the solidification process, and the solidification time for a large amount of sediment is long. For this reason, it is urgent to seek a material that can partially replace cement to prepare a curing agent specifically for solidifying sediment.

[0003] There is an urgent need to find a material that can replace cement to have a better solidification effect on the bottom mud and ensure environmental protection. In recent years, a large number of researchers have conducted research on the use of solid waste to solidify the bottom mud, such as using industrial waste residues to solidify the bottom mud with cement, which can not only partially replace cement as a raw material for solidifying the bottom mud, but also solve the problems of high energy consumption, high pollution and resource utilization of industrial waste residues of cement, but also promote the effective utilization of river and lake bottom mud and industrial solid waste, which is of great significance to environmental protection and full utilization of resources.

[0004] The rapid growth of the world's population, urbanization and industrialization inevitably lead to an increase in the amount of solid waste generated worldwide. The annual output of global solid waste is about 7-9 billion tons, and it is increasing sharply year by year. In 2016, the annual output of global urban solid waste was close to 2.01 billion tons, and it is expected to reach 3.4 billion tons by 2050. However, only about 30% of solid waste has been effectively treated. A large amount of industrial solid waste can only be piled up in material yards, occupying a large amount of land resources, and there are great ecological and environmental safety risks. In order to improve the level of resource utilization of industrial solid waste and reduce adverse effects on the environment, it is urgent to carry out research on the reuse of industrial solid waste. In this regard, some scholars have carried out the mixing of industrial solid waste with cement to prepare curing agent to solidify the bottom mud, so that the solidified bottom mud can be used for road fillers and other construction materials. This utilization method consumes a large amount of industrial solid waste, that is, it economically and ecologically treats a huge amount of river and lake bottom mud, and at the same time responds to the country's requirements to consume a large amount of industrial solid waste for resource utilization.

[0005] Current research is based on the physical properties of sediment to study the optimal dosage of industrial solid waste for sediment solidification, but ignores the interaction between soil minerals and solidifying agents, which results in the solidifying agent not having a good solidification effect on the sediment, and other soils with the same index properties have different solidification effects on the same solidifying agent. There are potential solidification active excitation components (SiO2, CaO, Al2O3 and Fe2O3) in industrial solid waste. The content of solidification active excitation components in industrial solid wastes with different contents and different industrial solid wastes is also different. The content of solidification active excitation components directly affects the solidification effect of the prepared solidifying agent on the sediment.

[0006] This phenomenon restricts the widespread use of solid waste in sediment reinforcement, and in the actual reinforcement process, it is difficult to achieve the expected solidification effect by simply adding a solidifying agent based on the physical properties of the sediment (such as water content, liquid limit, etc.). Therefore, how to reasonably configure industrial solid waste to prepare a solidifying agent that can have a good solidification effect on the sediment needs further in-depth research.

[0007] The active clay minerals in the sediment will interact with the hydration products generated by industrial solid waste during the hydration process, thereby affecting the mechanical properties of the solidified sediment. The content of active clay minerals in sediments in different regions is different, and different clay minerals have different dissolution reaction characteristics. However, the previous solid waste material component design framework did not consider the role of active clay minerals in the sediment in the solidification process, so there are certain limitations in the solid waste material design. The present invention incorporates the active clay mineral components in the sediment into the effective solidification components, and further improves the solid waste-based component design framework.

[0008] Since the bottom mud has the characteristics of high water content, low strength and high compressibility, it is difficult to use the bottom mud as roadbed filling material, which will bring some potential risks to the project. To solve this problem, there are many methods for reinforcing the bottom mud. At present, the most common methods include preloading, organic solidification and thermal solidification. These three methods can significantly improve the strength and stability of the soil, but they require a lot of energy and have a certain impact on the environment. Therefore, it is urgent to find a method that can have a significant solidification effect on the bottom mud, simple construction process, and can reduce energy consumption. Summary of the invention

[0009] The present invention aims to solve the solidification problem of active excitation components and sediment solidifying agents in sediment. The present invention is based on the potential solidification active excitation components in industrial solid waste through the solidification active excitation index and the aluminum rate, calcium rate and silicon rate control model, taking into account the activity of clay minerals in the clay component of the sediment; formulating a solidifying agent that can have a significant solidification effect on the sediment, and preparing a solidified sediment with simple construction process, green and environmental protection, and higher unconfined compressive strength.

[0010] In order to solve the above problems, the present application is implemented through the following technical solutions: A dynamic control method for ecological sediment solidification based on clay mineral composition comprises the following steps: S1. Drying and grinding the industrial solid waste for preparing the bottom mud solidifying agent to obtain respective industrial solid waste powders; S2. Measure the content of active excitation components of the industrial solid waste powder in step S1 by XRF i,j The curing activity excitation index η of industrial solid waste powder was measured by the activity index test i ; S3. Test the content of active components in clay minerals of sediment by oriented XRD * i,j , through w t-i,j , w 0-i,j Obtain the η of clay minerals in the sediment * i ; S4, step S2 in n i , ε i,j and n in step S3 * i , ε * i,j Substitute into the cement three-rate value control model to obtain the mass ratio of industrial solid waste in the sediment solidifier M i ; S5, adding the swelling agent component to the sediment curing agent configured in step S4 and the sediment preparation sample for curing, and after curing for 28 days, obtaining a sediment foundation preparation sample with a certain dry density, and determining the dosage of the swelling agent component according to the dry density; S6, according to the industrial solid waste mass ratio M in step S4 i The sludge curing agent is prepared according to the dosage of the expansion agent component in step S5, and the sludge is added to obtain the solidified soil samples for curing for 7 days, 28 days, and 60 days to obtain the solidified sludge of ordinary Portland cement with a certain dry density and unconfined compressive strength greater than that of ordinary Portland cement after curing for 7 days, 28 days, and 60 days.

[0011] The specific surface area of ​​the powder in step S1 is 300 m 2 / kg~400m 2 / kg.

[0012] In step S1, the industrial solid waste is selected from one or more of fly ash, yellow phosphorus slag, blast furnace slag and carbide slag; Among them, the active excitation components and the contents of each component of fly ash are 53.2% CaO, 8.2% Fe2O3, 22.4% SiO2, and 1.3% Al2O3 respectively; the active excitation components and the contents of each component of yellow phosphorus slag are 36.82% CaO, 4.3% Fe2O3, 37.24% SiO2, and 4.83% Al2O3 respectively; the active excitation components and the contents of each component of blast furnace slag are 37.2% CaO, 2.0% Fe2O3, 38.3% SiO2, and 16.4% Al2O3 respectively; the active excitation components and the contents of each component of carbide slag are 92.4% CaO, 0.4% Fe2O3, and 3.8% SiO2 respectively.

[0013] The industrial solid waste powder in step S2 is one or more of fly ash powder, yellow phosphorus slag powder, blast furnace slag powder and carbide slag powder.

[0014] The activity index test formula in step S2 is: i =δ i / B; Among them, δ i is the i-th industrial solid waste A i The test mortar has a 28-day compressive strength in MPa. B is the 28-day compressive strength of the cement-based comparison mortar, in MPa. When i=1, it indicates that the industrial solid waste is fly ash; when i=2, it indicates that the industrial solid waste is blast furnace slag; when i=3, it indicates that the industrial solid waste is carbide slag; when i=4, it indicates that the industrial solid waste is yellow phosphorus slag; When j is 1, it indicates that the latent curing active excitation component is SiO2, when j is 2, it indicates that the latent curing active excitation component is Fe2O3, when j is 3, it indicates that the latent curing active excitation component is Al2O3, when j is 4, it indicates that the latent curing active excitation component is CaO; η iIt represents the solidification activity excitation index of solid waste i in industrial solid waste; ε i,j It represents the chemical content of the potential solidification active component j in the i-th solid waste; Among them, ε 1,1 =22.4%, ε 1,2 =8.2%, ε 1,3 =1.3%, ε 1,4 =53.2%; ε 2,1 =38.3%, ε 2,2 =2%,ε 2,3 =16.4%, ε 2,4 =37.2%; ε 3,1 =3.8%, ε 3,2 =0.4%, ε 3,3 =0,ε 3,4 =92.4%; ε 4,1 =37.24%, ε 4,2 =4.3%, ε 4,3 =4.83%, ε 4,4 =36.82%; Among them, δ1=42.34MPa, δ2=45.08MPa, δ3=48.08MPa, δ4=46.17MPa, B=51.7MPa; eta1=0.819, eta2=0.872, eta3=0.93, eta4=0.893.

[0015] In the step S3, ε * i,j is the mass content of chemical components of potential solidification active component j in clay mineral i in the sediment; η * i is the reaction dissolution rate of the potential solidification active components in the clay minerals in the sediment; η * i =w t-i,j / w 0-i,j ; When i is 1, it indicates that the clay mineral is kaolinite, when i=2, it indicates that the clay mineral is montmorillonite, and when i is 3, it indicates that the clay mineral is illite; j is a natural number greater than zero: when j is 1, it indicates that the latent curing active exciting component is SiO2, when j is 2, it indicates that the latent curing active exciting component is Fe2O3, when j is 3, it indicates that the latent curing active exciting component is Al2O3, when j is 4, it indicates that the latent curing active exciting component is CaO; Preferably, in step S3, 0-i,j is the original content of j potential solidification active components in i clay minerals in the sediment; Where: w 0-1,1 =46.1%, w 0-1,3 =39.5%, w 0-1,2 =0.3%, w 0-1,4 =0.01%, w 0-2,1 =63.3%, w 0-2,3 =18.1%, w 0-2,2 =3.1%, w 0-2,4 =0.03%, w 0-3,1 =53.2%, w 0-3,3 =26.9%, w 0-3,2 =8.2%, w 0-3,4 =0.05%, w t-i,j is the reaction dissolution amount of j potential solidification active components in i clay mineral in the sediment; w t-1,1 =2.72%, w t-1,3 =2.33%, w t-1,2 =0.02%, w t-1,4 =0, w t-2,1 =7.60%, w t-2,3 =2.17%, w t-2,2 =0.37%, w t-2,4 =0, w t-3,1 =4.31%, w t-3,3 =2.18%, w t-3,2 =0.66%, w t-3,4 =0, Preferably, the clay minerals in the sludge in step S3 are kaolinite, montmorillonite and illite; wherein the kaolinite content is 16.4%, the montmorillonite content is 8.55%, and the illite content is 19.77%; SiO2 content in the active component of kaolinite * 1,1 =46.1%, Al2O3 content ε * 1,3 =39.5%, Fe2O3 content ε * 1,2 =0.3%, CaO content ε * 1,4 =0.01%; SiO2 content in the active component of montmorillonite *2,1 = 63.3%, the content of Al2O3 is ε * 2,3 = 18.1%, the content of Fe2O3 is ε * 2,2 = 3.1%, the content of CaO is ε * 2,4 = 0.03%; In the activator of illite, the content of SiO2 is ε * 3,1 = 53.2%, the content of Al2O3 is ε * 3,3 = 26.9%, the content of Fe2O3 is ε * 3,2 = 8.2%, the content of CaO is ε * 3,4 = 0.05%; Preferably, in step S3, η * 1 = 5.9%, η * 2 = 12.0%, η * 3 = 8.1%.

[0016] The control model of the three-ratio values of cement in step S4 is:

[0017]

[0018]

[0019] Among them, C i,j= η i × ε i,j C * i,j= η * i × ε * i,j ; The total number of types n of industrial solid wastes is 4, namely fly ash, yellow phosphorus slag, blast furnace slag, and carbide slag. In the three-ratio values of cement: SM is the silica modulus, 1.7 < SM < 2.7; IM is the alumina modulus, 0.9 < IM < 1.7; KH is the lime modulus, 0.9 < KH < 1.0; w IBP is the dosage of the curing agent; C i,j represents the activation content of the jth potential curing activation component in the ith industrial solid waste; C * i,j represents the activation content of the jth potential curing activation component in the ith clay mineral.

[0020] In step S4, M iis the mass ratio of solid waste i in industrial solid waste to the bottom mud solidifying agent; in terms of mass ratio, the ratio M i M fly ash: M yellow phosphorus slag: M blast furnace slag: M carbide slag = 21.4%~30%: 10%~16.7%: 19%~20%: 40%~42.9%.

[0021] In step S5, the expansion agent component is one of phosphogypsum, desulfurized gypsum, citric acid gypsum, titanium gypsum or fluorinated gypsum.

[0022] Among them, the components and contents contained in phosphogypsum are: CaO is 36.24%, Fe2O3 is 0.97%, SiO2 is 11.42%, MgO is 0.09%, Na2O is 1.03%, P2O5 is 0.02%, TiO2 is 0.17%, and SO3 is 43.22%.

[0023] Preferably, in step S5, the mass ratio of the bottom mud curing agent: the expansion agent component: the bottom mud = 0.1-0.2: 0.015-0.04: 1.

[0024] The dry density of the sample prepared from the bottom mud foundation in step S5 is 900 kg / m 3 -1600 kg / m 3 .

[0025] Preferably, in step S5, the mass ratio M of the bottom mud curing agent in step S4 is adjusted according to the determined mass fraction I of the swelling agent component. i They are M fly ash: M yellow phosphorus slag: M blast furnace slag: M carbide slag = 18.19~24: 8~14.2: 16~16.14: 32~36.47; Preferably, in step S5, the SiO2 content in the sludge is 73.23%, the Al2O3 content is 14.66%, the Fe2O3 content is 6.09%, the CaO content is 0.70%, the P2O5 content is 0.48%, the K2O content is 2.33%, the MnO content is 0.08%, the TiO2 content is 1.05%, and the SO3 content is 1.15%.

[0026] Preferably, in step S6, the unconfined compressive strength of ordinary Portland cement after curing for 7 days is 0.65 MPa, the unconfined compressive strength after curing for 28 days is 1.13 MPa, and the unconfined compressive strength after curing for 60 days is 1.25 MPa; Preferably, in step S6, the dry density of the solidified soil sample with a certain dry density is 900 kg / m 3 ~1200kg / m 3 .

[0027] Preferably, in step S6, the mass ratio of the bottom mud curing agent: the expansion agent component: the bottom mud = 0.1~0.2: 0.015~0.04: 1.

[0028] Preferably, in step S6, the expansion agent component is the same as that in step S5.

[0029] Preferably, the sludge in step S6 is the same as the sludge in step S5.

[0030] More preferably, the dosage of the expansion agent component corresponding to the first inflection point of the dry density variation curve in step S6 is a more economical dosage.

[0031] The steps and principles of the above-mentioned dynamic control method for ecological sediment solidification based on clay mineral composition are as follows: Step 1: Select raw materials The raw materials are industrial solid wastes with a large number of potential curing active components. The prepared curing agent can ensure that the bottom mud meets the corresponding engineering performance after curing; Step 2: Obtain the curing activity excitation content of potential curing activity excitation components in various types of industrial solid waste The curing active excitation components in various industrial solid wastes and clay minerals are analyzed. The potential curing active excitation components in industrial solid wastes and clay minerals are mainly four chemical substances, namely SiO2, CaO, Al2O3 and Fe2O3. According to the established curing active excitation content determination model, the active excitation content C of the potential curing active excitation components in various industrial solid wastes and clay minerals can be obtained. i,j and C * i,j , the above-mentioned curing excitation activity content determination model is: C i,j= η i *ε i,j C i,j represents the active excitation content of the jth potential solidification active excitation component in the i-th industrial solid waste; η i Represents the solidification activity excitation index of solid waste i in industrial solid waste; ε i,j It represents the chemical composition content of the potential solidification active component j in the i-th solid waste; j is a natural number greater than zero: when j is 1, it means that the potential solidification active component is SiO2, when j is 2, it means that the potential solidification active component is Fe2O3, when j is 3, it means that the potential solidification active component is Al2O3, when j is 4, it means that the potential solidification active component is CaO; C * i,j= η * i *ε * i,j C * i,j represents the active excitation content of the jth potential solidification active excitation component in the i-th clay mineral; η * i is the reaction dissolution rate of the potential solidification active components in the clay minerals in the sediment; ε * i,j is the mass content of chemical components of potential solidification active component j in clay mineral i in the sediment; j is a natural number greater than zero: when j is 1, it indicates that the potential solidification active component is SiO2; when j is 2, it indicates that the potential solidification active component is Fe2O3; when j is 3, it indicates that the potential solidification active component is Al2O3; when j is 4, it indicates that the potential solidification active component is CaO; Step 3: Obtain various types of industrial solid waste A i Mass ratio M i ; Taking clay mineral composition into consideration, the configuration ratio M of each industrial solid waste in the sediment reinforcement substrate is determined according to the constructed solidification activity excitation intensity control model. i , through the cement TCM control model (Three Chemical Moduli, i.e. three rate values), which specifically includes silicon rate (SM), aluminum rate (IM), and calcium rate (KH) control models.

[0032]

[0033]

[0034]

[0035] Among them, M i is the mass ratio of solid waste i in industrial solid waste to the bottom mud solidifying agent, w IBP is the curing agent dosage; Step 4: Prepare the bottom mud curing agent According to the various types of industrial solid waste A obtained in step 3 i Mass ratio M i Prepare the bottom mud solidifying agent at room temperature.

[0036] Step 5: Obtain the mass fraction of the expansion agent component I Add different mass ratios of expansive agent components to the sediment curing agent prepared in step 4, select specific sediment foundation to prepare samples for curing experiments, and after curing, measure the dry density of the samples, draw a dry density change curve, and determine the mass fraction of the expansive agent component I according to the change trend of the dry density curve.

[0037] Step 6: Prepare the bottom mud curing agent According to the various types of industrial solid waste A obtained in step three i Mass ratio M i The mass fraction I of the expansion agent component determined in step five can be compounded into the bottom mud solidifying agent at room temperature.

[0038] Preferably, the curing agent prepared in step 6 needs to further verify its curing performance (unconfined compressive strength). The specific steps are: the prepared curing agent is mixed with the bottom mud to prepare a sample, and the unconfined compressive strength of the sample is measured after curing for 28 days. If the strength does not meet the engineering requirements, it is necessary to increase the curing agent dosage w IBP , repeat steps three to six until the unconfined compressive strength of the bottom mud after solidifying with the configured curing agent meets the engineering performance requirements.

[0039] Preferably, the solidification activity excitation index η of the i-th industrial solid waste described in step 2 is obtained by an activity excitation index test. i : η i =δ i / B Where δ i Refers to the i-th type of industrial solid waste A i The test mortar has a 28-day compressive strength. B is the 28-day compressive strength of the cement-based reference mortar.

[0040] Preferably, the contents of active excitation components of kaolinite, montmorillonite and illite in the clay minerals of the sediment are tested by oriented XRD. * i,j , and then calculate the reaction dissolution rate η of the solidification active components of clay minerals in the sediment * i .

[0041] Preferably, the industrial by-product gypsum selected as the expansion agent component includes but is not limited to phosphogypsum, desulfurized gypsum, citric acid gypsum, titanium gypsum or fluorinated gypsum.

[0042] Preferably, there are four types of industrial solid waste in step one, specifically including fly ash, carbide slag, yellow phosphorus slag, and blast furnace slag, but not limited to these four types of industrial solid waste.

[0043] Preferably, the industrial solid waste in step 1 is pre-dried and ground into a specific surface area between 300m 2 / kg 400m 2 / kg of powder.

[0044] Preferably, in step 5, the dry density of the prepared solidified soil sample is measured after curing for 28 days.

[0045] Preferably, in step five, the mass fraction I of the expansion agent component is the content of the expansion agent component corresponding to the first inflection point in the dry density variation curve.

[0046] The present invention is a method for preparing a sediment reinforcement and curing agent for roadbed filling material. The ecological sediment curing dynamic control method based on clay mineral composition is used for various industrial solid wastes for sediment curing according to the following proportions, wherein the dosage of the curing agent in Example 1 is 10% of the sediment wet mass (the sediment wet mass is the mass of the original sediment obtained by on-site sampling, the same below), and the content of the curing agent is: 18.19 wt% fly ash, 15 wt% phosphogypsum, 14.2 wt% yellow phosphorus slag, 16.14 wt% blast furnace slag and 36.47 wt% carbide slag; the dosage of the curing agent in Example 2 is 20% of the sediment wet mass, and the content of the curing agent is: 24 wt% fly ash, 20 wt% phosphogypsum, 8 wt% yellow phosphorus slag, 16 wt% blast furnace slag and 32 wt% carbide slag.

[0047] The chemical composition contents of the corresponding potential solidification active excitation components in the above-mentioned fly ash, phosphogypsum, yellow phosphorus slag and blast furnace slag are shown in Table 1 below: Table 1 Potential active components and contents of solidification in various industrial solid wastes (%)

[0048] The chemical composition content of each potential curing active excitation component in Table 1 above is obtained through XRF measurement test.

[0049] Beneficial effects: Compared with the existing technology, the present invention has the following advantages: 1. The present invention takes into account the interaction between clay minerals and hydration products, combines the dissolution characteristics of different clay minerals, improves the existing solid waste component design framework, designs a sludge solidifying agent with good solidification effect, and provides a more effective utilization method for industrial solid waste. The solidified sludge can be used as roadbed filler and meets the requirements of highway roadbed and base specifications; 2. The method of preparing a sludge solidifying agent from industrial solid waste proposed in the present invention can achieve efficient utilization of industrial solid waste and significantly improve the strength of solidified sludge; 3. The present invention can absorb a large amount of industrial solid waste, reduce the amount of cement used, is green and environmentally friendly, has a simple process flow, is low in cost, can significantly improve the strength of solidified sludge, and is in line with the strategic goal of green and low-carbon development; 4. The present invention takes into account the interaction between clay minerals and hydration products in the sediment, comprehensively considers the composition, activity, fineness of solid waste and the reaction dissolution rate of potential solidification active excitation components in clay minerals, and on this basis optimizes the proportion of solid waste in the sediment solidifier, thereby promoting the hydration, volcanic ash and alkali excitation reaction performance of the solidified soil, which is not only conducive to the formation of cementitious products, but also can more accurately control the type and state of the reaction products, providing ideas for the utilization of solid waste-based solidified soil. The present invention can provide a way for the resource utilization and high-value utilization of industrial solid waste.

[0050] 5. Aiming at the deficiencies of existing solidification technology and curing agent preparation, the present invention optimizes the ratio of potential curing active stimulating components such as SiO2, CaO, Al2O3, and Fe2O3 in industrial solid waste (fly ash, carbide slag, yellow phosphorus slag, and blast furnace slag) to form a sediment solidifying agent. The potential curing active stimulating components in the sediment solidifying agent will activate the industrial solid waste. After the solid waste is reasonably formulated into a curing agent, the sediment solidification effect is obvious. Based on the concept of stimulating the activity of industrial solid waste by the potential curing active stimulating components in industrial solid waste, different contents of solid waste are configured to prepare a sediment reinforcement composite substrate. The method proposed by the present invention is economical and reasonable, the curing effect is controllable, the consumption of natural energy such as cement is greatly reduced, and industrial solid waste is used to replace part of cement to prepare a curing agent for sediment solidification, which is economical and environmentally friendly. The method establishes a design framework for sediment solidification material components from the gel and strength levels. A large amount of industrial solid wastes such as yellow phosphorus slag, blast furnace slag, and carbide slag are introduced into the preparation of sediment solidifiers. It is proposed to add corresponding industrial solid wastes according to the composition of clay minerals to stimulate the activity of sediment to the greatest extent. This method provides a more reasonable industrial solid waste design and selection for sediment solidification, as well as the amount of similar solid wastes. It not only improves the efficiency of sediment solidification, but also can recycle a large amount of industrial solid waste. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] Figure 1 This is the flow chart for preparing the bottom mud solidifying agent; Figure 2 It is the design framework diagram of industrial solid waste components; Figure 3 This is a diagram of the method for determining the optimal dosage of gypsum-based solid waste in the sediment; DETAILED DESCRIPTION Clay minerals are the clay component of sediment; in order to further clarify the purpose, technical scheme and advantages of the present invention, the present invention is described in detail below in conjunction with embodiments.

[0052] Step 1: Select raw materials The raw materials are industrial solid wastes with a large amount of potential solidification active excitation components, and the prepared solidifying agent can ensure that the bottom mud meets the corresponding engineering performance after solidification; Step 2: Obtain the curing activity excitation content of potential curing activity excitation components in various types of industrial solid waste The potential solidification active components in various industrial solid wastes and clay minerals are analyzed. The potential solidification active components in industrial solid wastes and clay minerals are mainly four chemical substances, namely SiO2, CaO, Al2O3 and Fe2O3. According to the established solidification active excitation content determination model, the active excitation content C of the potential solidification active components in various industrial solid wastes and clay minerals can be obtained. i,j and C * i,j ; The above-mentioned curing activity excitation content determination model is: C i,j= η i *ε i,j C i,j represents the active excitation content of the jth potential solidification active excitation component in the i-th industrial solid waste; η i Represents the solidification activity excitation index of solid waste i in industrial solid waste; ε i,j It represents the chemical composition content of the potential solidification active component j in the i-th solid waste; j is a natural number greater than zero: when j is 1, it means that the potential solidification active component is SiO2, when j is 2, it means that the potential solidification active component is Fe2O3, when j is 3, it means that the potential solidification active component is Al2O3, when j is 4, it means that the potential solidification active component is CaO; C * i,j= η * i *ε * i,j C * i,j represents the active excitation content of the jth potential solidification active excitation component in the i-th clay mineral; η * i is the reaction dissolution rate of the potential solidification active components in the clay minerals in the sediment; ε * i,j is the mass content of chemical components of potential solidification active component j in clay mineral i in the sediment; j is a natural number greater than zero: when j is 1, it indicates that the potential solidification active component is SiO2; when j is 2, it indicates that the potential solidification active component is Fe2O3; when j is 3, it indicates that the potential solidification active component is Al2O3; when j is 4, it indicates that the potential solidification active component is CaO; Step 3: Obtain the A of various types of industrial solid waste i Mass ratio M i Taking clay mineral composition into consideration, the configuration ratio M of each industrial solid waste in the sediment reinforcement substrate is determined according to the constructed solidification activity excitation intensity control model. i , through the cement TCM control model (Three Chemical Moduli, i.e. three rate values), which specifically includes the silicon rate (SM), aluminum rate (IM), and calcium rate (KH) control models;

[0053]

[0054]

[0055] Among them, M i is the mass ratio of solid waste i in industrial solid waste to the bottom mud solidifying agent, w IBP is the curing agent dosage.

[0056] Step 4: Prepare the bottom mud curing agent According to the various types of industrial solid waste A obtained in step 3 i Mass ratio M i Prepare the bottom mud solidifying agent at room temperature.

[0057] Step 5: Obtain the mass fraction of the expansion agent component I Add different mass ratios of expansion agent components to the curing agent prepared in step 4, select specific bottom mud foundation to prepare samples for curing experiments, and after curing, measure the dry density of the samples, draw a dry density change curve, and determine the mass fraction of each expansion agent component I according to the change trend of the dry density curve.

[0058] The by-product gypsum with expansion agent components added in step 5 includes but is not limited to phosphogypsum, desulfurized gypsum, citric acid gypsum, titanium gypsum or fluorinated gypsum. The addition of these by-product gypsums can react with the silicon-aluminum phase in an alkaline environment to generate hydration products. These hydration products will adhere to the surface of the sediment soil particles, causing the soil particles to aggregate and increase. The soil particles are wrapped by the hydrated calcium silicate (CSH) gel to fill the pores between the soil particles, and the soil can be tightly linked together. This shows that the reasonable configuration of industrial solid waste can maximize the role of potential solidification active excitation components and improve the solidification effect.

[0059] Step 6: Prepare the bottom mud solidifying agent.

[0060] According to the various types of industrial solid waste A obtained in step three i Mass ratio M i and the mass fraction I of the expansion agent component determined in step 5, the bottom mud solidifying agent can be compounded at room temperature; Preferably, the curing agent prepared in step 6 needs to further verify its curing performance (unconfined compressive strength). The specific steps are: the prepared curing agent is mixed with the bottom mud to prepare a sample, and the unconfined compressive strength of the sample is measured after curing for 28 days. If the strength does not meet the engineering requirements, it is necessary to increase the curing agent dosage w IBP Make corrections and repeat steps 3 to 6 to configure the curing agent until the unconfined compressive strength of the bottom mud after being cured by the corrected curing agent meets the engineering performance requirements.

[0061] Preferably, the solidification activity excitation index η of the i-th industrial solid waste described in step 2 is obtained by an activity excitation index test. i :η i =δ i / B; Where δ i Refers to the i-th type of industrial solid waste A i The test mortar has a 28-day compressive strength. B is the 28-day compressive strength of the cement-based reference mortar.

[0062] Preferably, the reaction dissolution rate η of the latent curing active excitation component in the clay mineral is * i Obtained by directional XRD.

[0063] In the following embodiments, if there is no special explanation, when conducting XRD test of oriented sheets, the preparation of oriented sheets specifically includes three steps. Step 1: Weigh 40 mg of the dried sample and place it in a 10 ml test tube, add 0.7 ml of distilled water and stir evenly, disperse the clay particles with ultrasound, let it stand for 30 minutes, pour the suspension on a glass slide, air-dry, and prepare a natural oriented sheet (N sheet); Step 2: Place the N sheet prepared in step 1 in an ethylene glycol vapor atmosphere for saturation treatment, the ethylene glycol vapor atmosphere is constant at 60°C, and the constant temperature time is not less than 8 hours; Step 3: Saturate the ethylene glycol sheet at 550°C for not less than 2.5 hours, and naturally cool to room temperature to obtain an oriented sheet.

[0064] If there is no special description, the curing condition is that the sample is placed in a curing box with a temperature of 20℃ and a humidity greater than 90%±3%. The content is the mass fraction.

[0065] Example 1 Industrial solid waste with large stockpiles and low utilization rates in Yichang City was selected, including fly ash, phosphogypsum, yellow phosphorus slag, blast furnace slag and carbide slag. Fly ash, blast furnace slag, carbide slag, phosphogypsum and yellow phosphorus slag were pre-dried and ground to a specific surface area of ​​300m 2 / kg~400m 2 / kg of powder is prepared for later use. The main chemical components of the solid waste are measured by XRF as shown in Table 2: Table 2 lists the main components and ignition loss of the solid waste (the remainder is other impurities, which will not be detailed).

[0066] Through the activity excitation index test, the results are shown in Table 3. The solidification activity excitation indexes η of fly ash, blast furnace slag, carbide slag and yellow phosphorus slag are measured i to be 0.819, 0.872, 0.93, and 0.893 respectively. According to the directional XRD, the reaction dissolution rates η of the potential solidification activity excitation components of clay minerals (kaolinite, montmorillonite and illite) are i * 5.9%, 12.0% and 8.1% respectively.

[0067] According to the cement TCM control model, with 1.7 < SM < 2.7, 0.9 < IM < 1.7, and 0.9 < KH < 1.0, the contents of industrial solid wastes added in the sediment solidifying agent are determined as follows: 21.4 wt% fly ash, 16.7 wt% yellow phosphorus slag, 19 wt% blast furnace slag, and 42.9 wt% carbide slag.

[0068] Table 2 Chemical compositions and contents (%) of solid wastes for preparing sediment solidifying agent

[0069] Table 3 Test results of activity indexes of industrial solid wastes

[0070] Select the sediment in Fuzhou. The mineral composition of the sediment is shown in Table 4, and a solidification experiment is carried out. Add the above-prepared solidifying agent to the sediment according to 10% of the wet mass of the sediment. Add 5 wt%, 10 wt%, 15 wt%, and 20 wt% of phosphogypsum as the expansion agent component respectively. After the prepared solidified soil specimens are cured under standard conditions for 28 days, draw the dry density change curve to determine the optimal dosage of the expansive component phosphogypsum I, and adjust the dosage of the solidifying agent obtained from the cement TCM control model. The adjusted dosage of the solidifying agent is 18.19 wt% fly ash, 14.2 wt% yellow phosphorus slag, 16.14 wt% blast furnace slag, 36.47 wt% carbide slag and 15 wt% phosphogypsum. The reaction dissolution amounts w t and reaction dissolution rates η i * are shown in Table 5.

[0071] Table 4 Minerals in Fuzhou sediment and mass fractions (%) of each component

[0072] Table 5 Reaction dissolution amounts of solidification activity excitation components of three clay minerals

[0073] The curing agent configured by the invention and the same amount of industrial solid waste (the amount added is 10% of the wet mass of the sludge) were added to the sludge respectively to solidify the sludge, and curing samples with different curing agents were prepared. The samples were cured in a standard curing room for 7d, 28d and 60d, and then their unconfined compressive strength was measured, which is listed in Table 6-1.

[0074] Table 6-1 Unconfined compressive strength of solidified sludge (MPa)

[0075] Example 2 Other method steps are the same as in Example 1, except that the amount of the bottom mud curing agent added is 20%, and the solid waste component ratio is: 30 wt% fly ash, 10 wt% yellow phosphorus slag, 20 wt% blast furnace slag, and 40 wt% carbide slag. The bottom mud in Fuzhou is selected for curing experiment, and the curing agent of the above configuration is added to the bottom mud. 5 wt%, 10 wt%, 15 wt%, and 20 wt% of phosphogypsum are added as the expansion agent component respectively, and the obtained solidified soil sample is subjected to standard curing for 28 days, and then a dry density variation curve is drawn to determine the dosage of the expansive component phosphogypsum I, and the curing agent dosage obtained by the cement TCM control model is adjusted, and the corrected curing agent dosage is 24 wt% fly ash, 8 wt% yellow phosphorus slag, 16 wt% blast furnace slag, 32 wt% carbide slag, and 20 wt% phosphogypsum. The curing agent configured by the invention and the same amount of industrial solid waste (the amount added is 20% of the wet mass of the sludge) were added to the sludge respectively to solidify the sludge, and curing samples with different curing agents were prepared. The samples were cured in a standard curing room for 7d, 28d and 60d, and then their unconfined compressive strength was measured, which is listed in Table 6-2.

[0076] In addition, when the content of the expansion agent component is selected in the embodiment of this patent, the dry density of the solidified soil is 900kg / m 3 -1600kg / m 3 The corresponding dosage of the expansion agent component has a beneficial effect on the strength of the solidified soil. Considering the economic benefits, the solidified soil density is selected as 900kg / m 3 -1200kg / m 3 It also has higher strength.

[0077] The industrial solid waste added to the curing agent needs to be pre-dried and ground to a specific surface area of ​​300m 2 / kg~400m 2 / kg of powder, the grinding cost should also be considered when configuring the curing agent. According to the market price, fly ash is 200 yuan / ton, blast furnace slag is 160 yuan / ton, carbide slag is 200 yuan / ton, phosphogypsum is 120 yuan / ton, yellow phosphorus slag is 140 yuan / ton, and ordinary Portland cement is 450 yuan / ton. After calculation, the curing agents in Example 1 and Example 2 of the present invention are 173 yuan / ton and 172.8 yuan / ton respectively. The strength of the bottom mud after 28 days of curing with the curing agent is 1.17 times and 1.14 times that of ordinary Portland cement respectively. It can be seen that the bottom mud curing agent has good economic benefits and curing effect.

[0078] Table 6-2 Unconfined compressive strength of solidified sludge (MPa)

[0079] In addition, the above are only preferred embodiments of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments, or change some of the technical features such as the types of industrial solid waste and sludge. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention shall be included in the protection scope of the present invention.

Claims

1. A dynamic control method for ecological sediment solidification based on clay mineral composition, characterized in that: The following steps are involved: S1. Drying and grinding the industrial solid waste for preparing the bottom mud solidifying agent to obtain respective industrial solid waste powders; S2. Measure the content of active excitation components of the industrial solid waste powder in step S1 by XRF i,j The curing activity excitation index η of industrial solid waste powder was measured by the activity index test i ; S3. Test the content of active components in clay minerals of sediment by oriented XRD * i,j , through w t-i,j , w 0-i,j Obtain the η of clay minerals in the sediment * i ; S4, step S2 in n i , ε i,j and n in step S3 * i , ε * i,j Substitute into the cement three-rate value control model to obtain the mass ratio of industrial solid waste in the sediment solidifier M i ; S5, adding the swelling agent component to the sediment curing agent configured in step S4 and the sediment preparation sample for curing, and after curing for 28 days, obtaining a sediment foundation preparation sample with a certain dry density, and determining the dosage of the swelling agent component according to the dry density; S6, according to the industrial solid waste mass ratio M in step S4 i The sludge curing agent is prepared according to the dosage of the expansion agent component in step S5, and the sludge is added to obtain the solidified soil samples for curing for 7 days, 28 days, and 60 days to obtain the solidified sludge of ordinary Portland cement with a certain dry density and unconfined compressive strength greater than that of ordinary Portland cement after curing for 7 days, 28 days, and 60 days.

2. According to claim 1, a dynamic control method for ecological sediment solidification based on clay mineral composition is characterized in that: The specific surface area of ​​the powder in step S1 is 300 m 2 / kg~400m 2 / kg.

3. According to claim 1, a dynamic control method for ecological sediment solidification based on clay mineral composition is characterized in that: In step S1, the industrial solid waste is selected from one or more of fly ash, yellow phosphorus slag, blast furnace slag and carbide slag; Among them, the active excitation components and the contents of each component of fly ash are 53.2% CaO, 8.2% Fe2O3, 22.4% SiO2, and 1.3% Al2O3 respectively; the active excitation components and the contents of each component of yellow phosphorus slag are 36.82% CaO, 4.3% Fe2O3, 37.24% SiO2, and 4.83% Al2O3 respectively; the active excitation components and the contents of each component of blast furnace slag are 37.2% CaO, 2.0% Fe2O3, 38.3% SiO2, and 16.4% Al2O3 respectively; the active excitation components and the contents of each component of carbide slag are 92.4% CaO, 0.4% Fe2O3, and 3.8% SiO2 respectively.

4. According to claim 1, a dynamic control method for ecological sediment solidification based on clay mineral composition is characterized in that: The industrial solid waste powder in step S2 is one or more of fly ash powder, yellow phosphorus slag powder, blast furnace slag powder and carbide slag powder.

5. According to claim 1, a dynamic control method for ecological sediment solidification based on clay mineral composition is characterized in that: The activity index test formula in step S2 is: i =δ i / B; Among them, δ i is the i-th industrial solid waste A i The test mortar has a 28-day compressive strength in MPa. B is the 28-day compressive strength of the cement-based comparison mortar, in MPa. When i=1, it indicates that the industrial solid waste is fly ash; when i=2, it indicates that the industrial solid waste is blast furnace slag; when i=3, it indicates that the industrial solid waste is carbide slag; when i=4, it indicates that the industrial solid waste is yellow phosphorus slag; When j is 1, it indicates that the latent curing active excitation component is SiO2, when j is 2, it indicates that the latent curing active excitation component is Fe2O3, when j is 3, it indicates that the latent curing active excitation component is Al2O3, when j is 4, it indicates that the latent curing active excitation component is CaO; η i It represents the solidification activity excitation index of solid waste i in industrial solid waste; ε i,j It represents the chemical composition content of the potential solidification active excitation component j in the i-th type of solid waste.

6. According to claim 1, a dynamic control method for ecological sediment solidification based on clay mineral composition is characterized in that: In the step S3, ε * i,j is the mass content of chemical components of potential solidification active component j in clay mineral i in the sediment; η * i is the reaction dissolution rate of the potential solidification active components in the clay minerals in the sediment; or * i =w t-i,j / w 0-i,j ; When i is 1, it indicates that the clay mineral is kaolinite, when i=2, it indicates that the clay mineral is montmorillonite, and when i is 3, it indicates that the clay mineral is illite; j is a natural number greater than zero: when j is 1, it indicates that the potential curing active excitation component is SiO2; when j is 2, it indicates that the potential curing active excitation component is Fe2O3; when j is 3, it indicates that the potential curing active excitation component is Al2O3; when j is 4, it indicates that the potential curing active excitation component is CaO.

7. According to claim 1, a dynamic control method for ecological sediment solidification based on clay mineral composition is characterized in that: The cement three-rate value control model in step S4 is: Among them, C i,j= η i ×ε i,j , C * i,j= η * i ×ε * i,j ; The total number of types n of industrial solid wastes is 4, namely fly ash, yellow phosphorus slag, blast furnace slag, and carbide slag. Among the three modulus values of cement: SM is the silica modulus, 1.7 < SM < 2.7; IM is the alumina modulus, 0.9 < IM < 1.7; KH is the lime modulus, 0.9 < KH < 1.0; w IBP is the dosage of the curing agent; C i,j It represents the active excitation content of the jth potential solidification active excitation component in the i-th industrial solid waste; C * i,j It represents the active excitation content of the jth potential solidification active excitation component in the i-th clay mineral.

8. According to claim 1, a dynamic control method for ecological sediment solidification based on clay mineral composition is characterized in that: In step S4, i is the mass ratio of solid waste i in industrial solid waste in the sludge solidifying agent; In terms of mass ratio, the proportion of M in the sediment solidifying agent is i M fly ash: M yellow phosphorus slag: M blast furnace slag: M carbide slag = 21.4%~30%: 10%~16.7%: 19%~20%: 40%~42.9%.

9. The method for dynamic regulation of ecological sediment solidification based on clay mineral composition according to claim 1, characterized in that: In step S5, the expansion agent component is one of phosphogypsum, desulfurized gypsum, citric acid gypsum, titanium gypsum or fluorinated gypsum.

10. The method for dynamic regulation of ecological sediment solidification based on clay mineral composition according to claim 1, characterized in that: The dry density of the sample prepared from the bottom mud foundation in step S5 is 900 kg / m 3 -1600 kg / m 3 .

Citation Information

Patent Citations

  • Soft foundation reinforcing composite base material and method for preparing soft foundation reinforcing composite base material through normal-temperature recombination of multiple kinds of solid waste

    CN113698167A

Cited By

  • Preparation method of multi-source sludge solidified soil

    CN119954483A

  • All-solid-waste self-excitation muck slurry and preparation method thereof

    CN122277172A