Integrated construction method for milling section steel fiber reinforced carborundum terrace
By using an integrated construction method for milled steel fiber reinforced diamond abrasive flooring, common quality problems in traditional steel mesh diamond abrasive flooring construction have been solved, resulting in shorter construction time, improved wear resistance, and reduced construction costs.
Patent Information
- Application Number
- CN202410997197.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-29
AI Technical Summary
Traditional steel mesh and diamond abrasive wear-resistant flooring is prone to common quality problems such as hollowness, peeling, cracks, and color difference during construction. It involves many procedures, is not conducive to shortening the construction period, and has high construction costs.
The integrated construction method of milled steel fiber reinforced carborundum flooring is adopted, which includes a carborundum layer, a steel fiber concrete layer, a thick soil cushion layer and a compacted plain soil layer. Through steps such as elevation measurement, preparation and pouring of steel fiber concrete, spreading of carborundum, cutting of expansion joints and curing, a concrete structure with uniformly distributed milled steel fibers is formed.
It solves the common quality problems of traditional methods, shortens the construction period, reduces construction costs, and improves the wear resistance and structural durability of the floor.
Smart Images

Figure CN119041653A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of floor construction, and in particular to an integrated construction method for a milled steel fiber reinforced diamond sand floor. Background Art
[0002] Diamond wear-resistant floor has the advantages of wear resistance, impact resistance, high strength, easy repair, dust suppression, environmental protection, simple process and various colors. It is constantly used in parking lots of residential buildings, parking lots of large shopping malls, logistics storage and transportation, product processing workshops and other building floors.
[0003] The traditional steel mesh diamond wear-resistant floor is constructed with a 5cm thick wear-resistant floor decoration layer at the end of the construction. This process is constructed to 1 / 3 of the surface layer during the steel mesh binding and pouring process, but it is easy to produce hollowing, peeling, cracks, color difference and other quality problems. More importantly, there are many processes, which is not conducive to shortening the construction period and the construction cost is high. Therefore, it is a technical problem that people in this field urgently need to solve. Summary of the invention
[0004] Technical problem to be solved: In order to overcome the above shortcomings, an integrated construction method for milling steel fiber reinforced diamond abrasive floor is provided.
[0005] The technical solution is: an integrated structure of milled steel fiber reinforced corundum floor, which includes, from top to bottom, a corundum layer, a steel fiber concrete layer, a thick soil cushion layer and a plain soil ramming layer; the steel fiber concrete layer is formed by evenly distributing milled steel fibers in concrete and solidifying them.
[0006] The integrated construction method of milling steel fiber reinforced diamond sand floor includes the following steps:
[0007] 1) Elevation measurement: The structural elevation control points are measured from the leveling control points of the construction site, and elevation control points are set with a vertical and horizontal spacing of no more than 3m; the construction site is completed with a rammed earth layer and a thick soil cushion layer in accordance with standard specifications, and the compaction coefficient of the thick soil cushion layer is not less than 0.97; the compaction coefficient of the rammed earth layer is not less than 0.94.
[0008] 2) Preparation of steel fiber concrete: 20kg / m 3 Add the milled steel fibers into the concrete in a certain proportion and mix well to ensure that the steel fibers are evenly dispersed in the mixture;
[0009] 3) Steel fiber concrete pouring: pour steel fiber concrete on the thick soil cushion, use a laser leveling machine for paving, vibrating, leveling and slope finding, and ensure that the flatness of the steel fiber concrete does not exceed 3mm / m;
[0010] 4) Emery paving: After the initial setting and before the final setting of the steel fiber concrete, evenly spread 2 / 3 of the emery material on it, and smooth it for the first time after the material absorbs the moisture in the steel fiber concrete;
[0011] Spread the remaining 1 / 3 of the diamond abrasive material evenly perpendicular to the first spreading direction, and perform the second smoothing;
[0012] 5) Cutting expansion joints: Cut expansion joints within 24-36 hours before the final setting of concrete to ensure that there are no irregular cracks on the floor surface;
[0013] 6) Maintenance: Start watering and covering with film within 12 hours after the concrete pouring is completed to keep the concrete moist. The maintenance time is not less than 14 days;
[0014] 7) Filling the seams with sealant: Remove loose particles and dust from the cut seams, and use polyurethane sealant to fill the seams to ensure that the seams are beautiful and do not contaminate the ground.
[0015] Preferably, the method for preparing steel fiber concrete in step 2) comprises the following raw materials:
[0016] Cement, fine aggregate, coarse aggregate, milled steel fiber; and water reducer, expansion agent and water, wherein the water reducer is 1.5-2% of the weight of cement, the expansion agent is 2-3% of the weight of cement, and the water is 35-40% of the weight of cement;
[0017] The preparation method of the steel fiber concrete comprises the following steps:
[0018] 1) Dry mix cement, fine aggregate, coarse aggregate, silica fume and expansion agent to ensure uniform distribution;
[0019] 2) Add water and water reducing agent and continue stirring to ensure uniform mixing;
[0020] 3) Finally, add the milled steel fibers and continue stirring to ensure that the milled steel fibers are evenly distributed in the concrete.
[0021] Preferably, the raw material ratio of each component is: cement 400kg / m 3 , fine aggregate 600kg / m 3 , coarse aggregate 1200kg / m 3 , Milling steel fiber 20-25kg / m 3 .
[0022] Preferably, the step 7) of maintenance further includes: after the maintenance is completed, spraying a curing agent and performing multiple grinding and polishing to make the floor surface bright and wear-resistant.
[0023] Beneficial effects: 1. Milled steel fibers are used instead of traditional steel meshes, eliminating the need for steel bar tying processes and shortening construction time.
[0024] 2. Milling steel fiber has high tensile strength, good toughness and dispersibility. When mixed and dispersed with concrete, it improves the crack resistance, tensile and shear resistance of the mixture. In addition, the diamond wear-resistant material is spread on the surface of steel fiber concrete, which enhances the wear resistance and structural durability of the floor. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a cross-sectional view of the integrated structure of the milled steel fiber reinforced diamond abrasive floor in the present invention.
[0026] Figure 2 The present invention is a flow chart of the integrated construction method of the milling steel fiber reinforced diamond abrasive floor. DETAILED DESCRIPTION
[0027] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments, but is not intended to limit the present invention.
[0028] like Figure 1 As shown, the integrated structure of the milled steel fiber reinforced corundum floor comprises, from top to bottom, a corundum layer, a steel fiber concrete layer, a thick soil cushion layer and a plain soil ramming layer; the steel fiber concrete layer is formed by evenly distributing the milled steel fibers in the concrete and solidifying them.
[0029] like Figure 2 As shown, the integrated construction method of milling steel fiber reinforced diamond abrasive flooring includes the following steps:
[0030] 1) Elevation measurement: The structural elevation control points are measured from the leveling control points of the construction site, and elevation control points are set with a vertical and horizontal spacing of no more than 3m; the construction site is completed with a rammed earth layer and a thick soil cushion layer in accordance with standard specifications, and the compaction coefficient of the thick soil cushion layer is not less than 0.97; the compaction coefficient of the rammed earth layer is not less than 0.94.
[0031] The structural elevation control point is measured from the leveling control point of the construction unit, which is generally a 1-meter control point. This is used as the basis for the finished floor surface height. Elevation control points with a vertical and horizontal spacing of no more than 3m are evenly set on the vertical components and the board surface. After completion, the project department shall conduct a special review and acceptance and keep written records to ensure that the concrete surface layer is flat and consistent. At the same time, the inspection and control are strengthened during the concrete distribution and pouring process, and a set of laser level and level are set up to conduct timely inspection and review during the pouring process.
[0032] In the specific implementation process, it also includes selecting armored seams that are suitable for the floor height standard and placing them at the location where they need to be erected; taking a center point at each end of the erection location and pulling a line between the two points. Appropriately adjust the position of the armored seam so that the middle seam is parallel to the pull line, and pay special attention to ensuring that the middle seam is in a straight line when two armored seams are connected to ensure that the seam is beautiful; place a tower ruler on the upper surface of the construction joint, and fine-tune the height through the level to achieve the set elevation; on the side after the armored seam is cast, short steel bars are driven in every 60cm for fixation; the sleeve is driven into the force transmission plate on the side of the armored seam to be cast, and the installation of the armored seam is completed.
[0033] 2) Steel fiber concrete preparation: 20-25kg / m 3 Add the milled steel fibers into the concrete in a certain proportion and mix well to ensure that the steel fibers are evenly dispersed in the mixture.
[0034] Among them, the milling steel fiber: length: 32.0mm±2.0mm; width: 2.6mm±1.2mm; aspect ratio: 35-45; effective aspect ratio 120; tensile strength: 600-1000MPa;
[0035] 3) Steel fiber concrete pouring: Pour steel fiber concrete on the thick soil cushion layer, and use a laser leveling machine to spread, vibrate, level and slope to ensure that the flatness of the steel fiber concrete does not exceed 3mm / m.
[0036] During the specific implementation process, the concrete needs to be vibrated and compacted until the slurry comes out during pouring and vibration. At the same time, the vibration time should not be too long, otherwise the steel fibers will accumulate in the bottom layer. The laser leveling machine is used to spread the concrete (the flatness reaches 2m±3mm), and the elevation is detected by the laser leveling machine transmitter. The laser leveling machine is used for automatic construction of slope, vibration, leveling and leveling. Small vibrating scrapers are used to level and vibrate the wall edges, column bases and parts that cannot be leveled by the laser leveling machine. After the laser leveling machine is completed, a 6m aluminum alloy ruler is used to adjust the flatness. The slump of the concrete is strictly controlled to 140-160mm, and it is strictly forbidden to add water during the process. The amount of fly ash used in the concrete is strictly controlled to avoid affecting the quality of the concrete work.
[0037] 4) Emery paving: After the initial setting and before the final setting of the steel fiber concrete, evenly spread 2 / 3 of the emery material on it, and smooth it for the first time after the material absorbs the moisture in the steel fiber concrete;
[0038] Spread the remaining 1 / 3 of the emery material evenly perpendicular to the first spreading direction and perform the second smoothing.
[0039] In the specific implementation process, after the concrete is poured, the emery is spread and the exudate should be removed, and the slurry should be raised and leveled. After the initial setting and before the final setting of the concrete, emery is spread twice and emery construction with different proportions is carried out for different functional areas of the floor; the first time, 2 / 3 of the emery material is spread evenly on the concrete surface by machinery, and the first leveling is started after the material absorbs the moisture in the concrete, the surface becomes damp and the color becomes gray; then the remaining 1 / 3 of the material is spread manually on the concrete surface, and the spreading direction is perpendicular to the first time, and then the second leveling work is carried out;
[0040] Finally, use an electric grinder to grind and polish the surface of the diamond layer to ensure that the surface is flat and smooth;
[0041] 5) Cutting expansion joints: Cut expansion joints within 24-36 hours before the final setting of concrete to ensure that there are no irregular cracks on the floor surface;
[0042] During the specific implementation process, the expansion joints are cut within 24h-36h of concrete pouring, and the diamond joints are cut on the column edge; first, the compartment joints are trimmed to ensure that the compartment joints are straight; second, the false joints are cut, and the compartment joints are sawed according to the requirements of ≤6m in the vertical and horizontal directions. The sawing seams must be marked, and the false seams are 5mm wide, 25-30mm deep and not less than 1 / 3 of the leveling layer thickness. Before cutting large areas, a trial cut should be carried out, and the cutting edges should not be broken, and the spacing should not be greater than 6m×6m.
[0043] 6) Maintenance: Start watering and covering with film within 12 hours after the concrete pouring is completed to keep the concrete moist. The maintenance time should be no less than 7 days.
[0044] In the specific implementation process, the geotextile should be covered and watered during the curing period. The number of watering curing should be enough to keep the concrete moist. In the first three days, watering should be ensured at least three times a day. All exposed surfaces of the concrete should be tightly covered. And sufficient curing should be carried out every day within 7 days.
[0045] 7) Filling the seams with sealant: Remove loose particles and dust from the cut seams, and use polyurethane sealant to fill the seams to ensure that the seams are beautiful and do not contaminate the ground.
[0046] During the specific implementation process, after the floor maintenance is completed, all loose particles and dust in the cut joints are removed; the joints are filled with long-lasting elastic and fast-curing polyurethane sealant; avoid introducing air when applying the sealant; the joints are filled as beautifully as possible without polluting the ground. When filling the joints with glue, masking tape is pasted on both sides of the gap to ensure that the glue thickness is not less than 5mm.
[0047] In a more preferred embodiment, the method for preparing steel fiber concrete in step 2) comprises the following raw materials:
[0048] Cement 400kg / m 3 , fine aggregate 600kg / m3 , coarse aggregate 1200kg / m 3 , Milling steel fiber 20-25kg / m 3 ; And a water reducing agent, an expansion agent and water, the water reducing agent is 1.5-2% of the weight of cement, the expansion agent is 2-3% of the weight of cement, and the water is 35-40% of the weight of cement;
[0049] The preparation method of the steel fiber concrete comprises the following steps:
[0050] 1) Dry mix cement, fine aggregate, coarse aggregate, silica fume and expansion agent to ensure uniform distribution;
[0051] 2) Add water and water reducing agent and continue stirring to ensure uniform mixing;
[0052] 3) Finally, add the milled steel fibers and continue stirring to ensure that the milled steel fibers are evenly distributed in the concrete.
[0053] In a more preferred embodiment, the step 6) of maintenance further includes: after the maintenance is completed, spraying a curing agent and performing multiple grinding and polishing to make the floor surface bright and wear-resistant.
[0054] During the specific implementation process, after the ground is completely dry, spray the curing agent evenly on the floor for the second time (0.15kg / ㎡), use 500 mesh-800 mesh-1000 mesh-1500 mesh resin grinding discs to cross-grind until the ground is polished, and then use 2000 mesh resin grinding discs to grind and polish the ground until the ground is clear and bright; finally, use a scouring pad or polishing sheet to polish the ground until the ground has a high-gloss effect.
[0055] The integrated construction method of milled steel fiber reinforced diamond abrasive floor in the above embodiments of the present invention can be applied to various residential parking lots, large shopping malls, parking lots, logistics storage and transportation, product processing workshops and other buildings that have high requirements for ground wear resistance.
[0056] The above embodiments are provided for persons familiar with the art to implement or use the present invention. Persons familiar with the art can make various modifications or changes to the above embodiments without departing from the inventive concept of the present invention. Therefore, the protection scope of the present invention is not limited to the above embodiments, but should be the maximum scope of the innovative features mentioned in the claims.
Claims
1. The integrated construction method of milling steel fiber reinforced diamond floor is characterized by: It includes, from top to bottom, a corundum layer, a steel fiber concrete layer, a thick soil cushion layer and a plain soil ramming layer; the steel fiber concrete layer is formed by uniformly distributing milling steel fibers in concrete and solidifying them.
2. The integrated construction method of milling steel fiber reinforced diamond floor according to claim 1 is characterized in that: The following steps are involved: 1) Elevation measurement: The structural elevation control points are measured from the leveling control points of the construction site, and the elevation control points are set with a vertical and horizontal spacing of no more than 3m; the construction site is completed with a rammed earth layer and a thick soil cushion layer in accordance with standard specifications, and the compaction coefficient of the thick soil cushion layer is not less than 0.97; the compaction coefficient of the rammed earth layer is not less than 0.94; 2) Preparation of steel fiber concrete: 20kg / m 3 Add the milled steel fibers into the concrete in a certain proportion and mix well to ensure that the steel fibers are evenly dispersed in the mixture; 3) Steel fiber concrete pouring: pour steel fiber concrete on the thick soil cushion, use a laser leveling machine for paving, vibrating, leveling and slope finding, and ensure that the flatness of the steel fiber concrete does not exceed 3mm / m; 4) Emery paving: After the initial setting and before the final setting of the steel fiber concrete, evenly spread 2 / 3 of the emery material on it, and smooth it for the first time after the material absorbs the moisture in the steel fiber concrete; Spread the remaining 1 / 3 of the diamond abrasive material evenly perpendicular to the first spreading direction, and perform the second smoothing; 5) Cutting expansion joints: Cut expansion joints within 24-36 hours before the final setting of concrete to ensure that there are no irregular cracks on the floor surface; 6) Maintenance: Start watering and covering with film within 12 hours after the concrete pouring is completed to keep the concrete moist. The maintenance time is not less than 14 days; 7) Filling the seams with sealant: Remove loose particles and dust from the cut seams, and use polyurethane sealant to fill the seams to ensure that the seams are beautiful and do not contaminate the ground.
3. The integrated construction method of milling steel fiber reinforced diamond floor according to claim 2 is characterized in that: The method for preparing steel fiber concrete in step 2) comprises the following raw materials: Cement, fine aggregate, coarse aggregate, milled steel fiber; and water reducer, expansion agent and water, wherein the water reducer is 1.5-2% of the weight of cement, the expansion agent is 2-3% of the weight of cement, and the water is 35-40% of the weight of cement.
4. The integrated construction method of milling steel fiber reinforced diamond floor according to claim 3 is characterized in that: The raw material ratio of each component is: cement 400kg / m 3 , fine aggregate 600kg / m 3 , coarse aggregate 1200kg / m 3 , Milling steel fiber 20-25kg / m 3 .
5. The integrated construction method of milling steel fiber reinforced diamond floor according to claim 3 is characterized in that: The preparation method of the steel fiber concrete comprises the following steps: 1) Dry mix cement, fine aggregate, coarse aggregate, silica fume and expansion agent to ensure uniform distribution; 2) Add water and water reducing agent and continue stirring to ensure uniform mixing; 3) Finally, add the milled steel fibers and continue stirring to ensure that the milled steel fibers are evenly distributed in the concrete.
6. The integrated construction method of milling steel fiber reinforced diamond floor according to claim 2 is characterized in that: The step 7) of maintenance also includes: after the maintenance is completed, spraying a curing agent and performing multiple grinding and polishing to make the floor surface bright and wear-resistant.