Flexible stretchable electrochromic device and preparation method thereof

By using a combination technology of hydrogel substrates and silver nanowires/tungsten oxide quantum dots in flexible electrochromic devices, a multi-layer composite structure is constructed, which solves the performance problems of the device in arbitrary angle bending and large-scale stretching. , improves response speed and cycle stability and extends device life.

CN119045251AActive Publication Date: 2024-11-29SUZHOU UNIV

Patent Information

Application Number
CN202410468879.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-04-18
Publication Date
2024-11-29
Estimated Expiration
2044-04-18

AI Technical Summary

Technical Problem

Existing flexible electrochromic devices cannot have the properties of arbitrary angle bending and large-scale stretching, fast response speed, and repeat stretching cycle stability. In the long-term electrochemical cycle environment, silver nanowire electrodes are easily oxidized, resulting in Performance deteriorates.

Method used

The hydrogel-based flexible substrate is prepared using raw materials such as acrylamide, acrylic acid, 2-acrylamide-2-methylpropane sulfonic acid, lithium chloride, etc., and combined with silver nanowires, tungsten oxide quantum dots and other materials, and spin coating The conductive electrode and electrochromic layer were prepared by drop coating technology to construct a multi-layer composite structure.

Benefits of technology

The 200% tensile elongation, fast response speed and good optical contrast of flexible electrochromic devices are achieved, and the tensile cycle stability is improved by 2.5 times, extending the device's service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119045251A_ABST
    Figure CN119045251A_ABST
Patent Text Reader

Abstract

The invention discloses a flexible stretchable electrochromic device and a preparation method thereof. The flexible stretchable electrochromic device comprises a hydrogel-based flexible substrate, an electrochromic layer and a conductive electrode layer, the hydrogel-based flexible substrate is 2-acrylamido-2-methylpropanesulfonic acid / acrylamide / acrylic acid / lithium chloride hydrogel with excellent transparency, stretchability and ionic conductivity and acrylamide hydrogel with excellent transparency and stretchability, and the electrochromic layer is formed by mixing a tungsten oxide quantum dot solution prepared by a hydrothermal method and poly (3, 4-dichlorophenyl)-1, 2, 3, 4-tetramethyl-1, 3-pentanediol monoisobutyrate). The conductive electrode layer is a uniform composite layer formed by mixing a poly 3, 4-ethylenedioxythiophene-polystyrolsulfon acid solution and then dispensing, and the conductive electrode layer is prepared by compounding a silver nanowire / poly 3, 4-ethylenedioxythiophene-polystyrolsulfon acid solution and then carrying out spin coating on the compounded silver nanowire / poly 3, 4-ethylenedioxythiophene-polystyrolsulfon acid solution. According to the flexible stretchable electrochromic device, the flexible stretchable electrochromic device has excellent flexibility (1000 times of cyclic stretching under the tensile elongation of 200%), high response speed and good optical contrast (DT = 34%).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of electrochromic device preparation, and in particular to a flexible and stretchable electrochromic device and a preparation method thereof. Background Art

[0002] As an emerging intelligent soft electronic device, flexible electrochromic devices have the characteristics of high controllability, fast response speed and low power consumption. They can realize rapid information interaction and display between humans and machines. They have broad application prospects in the fields of smart wearable devices, electronic skin and energy storage devices. They provide a feasible strategy for the development of next-generation electronic products and have received widespread attention. However, the flexible electrochromic devices currently prepared are limited by flexible substrates and conductive electrodes, and can only achieve bending at a certain angle and a small degree of stretching. At the same time, due to the complexity of the device structure, when subjected to a large degree of deformation, there is a large modulus mismatch between the two interconnected material layers, the mechanical and chemical compatibility of the interface is poor, and stratification is easy to occur, which affects the response speed and optical contrast of the device, resulting in low comprehensive performance of the electrochromic device. Therefore, in order to make the electrochromic device comfortable, conformal and durable when integrated into wearable devices or applied on non-planar surfaces, it is very necessary to develop visual, personalized and simplified stretchable or deformable electrochromic devices.

[0003] Flexible conductive electrodes with high transparency, conductivity, excellent mechanical properties and electrochemical stability are key factors in constructing stretchable electrochromic devices. At present, stretchable conductive electrodes are usually prepared by mixing conductive materials with elastomers or polymers or attaching conductive materials to flexible substrates by various methods (drip coating, spin coating, spray coating, scraping, etc.). Among the conductive materials, metal nanowires (silver nanowires, gold nanowires) and conductive polymers (poly (3,4-ethylenedioxythiophene-polystyrene sulfonic acid, polyaniline, polypyrrole, etc.) are usually used as active conductive materials due to their excellent flexibility, conductivity and electrochemical stability. Among them, silver nanowire networks are considered to be a promising conductive material due to their high transparency and excellent conductivity. However, bare silver nanowires are easily oxidized in long-term electrochemical cycling environments or humid environments, resulting in rapid deterioration of the performance of electrodes with silver nanowire networks. Flexible substrates are another key factor in realizing stretchable electrochromic devices. Currently, commonly used flexible substrates include polydimethylsiloxane, hydrogenated styrene-butadiene-styrene (SEBS) triblock copolymer, Ecoflex, polyurethane and fabrics with good elasticity, all of which show excellent transparency, flexibility and chemical stability. However, it is often necessary to adopt modification treatment, functional group addition, and multiple material composites to achieve the preparation of flexible substrates with high elongation, excellent ductility and adaptability, so that their Young's modulus can match that of most soft tissues and reduce the mechanical mismatch at the interface. Summary of the invention

[0004] The purpose of the present invention is to solve the technical problems that the existing flexible electrochromic devices cannot have both arbitrary angle bending and large degree of stretching, fast response speed, repeated stretching cycle stability, etc., thereby providing a flexible electrochromic device and its preparation method. In the present invention, the flexible stretchable electrochromic device has excellent flexibility (200% tensile elongation cyclic stretching 1000 times), fast response speed and good optical contrast (DT=34%). Compared with other related reported devices, while maintaining its electrochromic performance, the tensile elongation of the device is increased by about 4 times, and the tensile cycle stability is increased by about 2.5 times.

[0005] The present invention adopts the following technical solution: A method for preparing a flexible and stretchable electrochromic device comprises the following steps: (1) Using acrylamide, acrylic acid, 2-acrylamide-2-methylpropane sulfonic acid and lithium chloride as raw materials, a 2-acrylamide-2-methylpropane sulfonic acid / acrylamide / acrylic acid / lithium chloride hydrogel-based flexible substrate was prepared; (2) Using acrylamide as raw material, preparing an acrylamide hydrogel-based flexible substrate; (3) using ethylene glycol, isopropanol, poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid) solution, silver nanowires and surfactant as raw materials to form a silver nanowire / poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid composite solution; (4) preparing a silver nanowire / poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid) composite solution into a conductive electrode layer, and then attaching it to an acrylamide hydrogel flexible substrate to form a conductive electrode layer on the surface of the acrylamide hydrogel flexible substrate; (5) mixing tungsten oxide quantum dots with poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid) solution and surfactant to prepare tungsten oxide quantum dots / poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid electrochromic solution; (6) The electrochromic layer is prepared from a tungsten oxide quantum dot / poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid electrochromic solution, and then attached to a 2-acrylamide-2-methylpropane sulfonic acid / acrylamide / acrylic acid / lithium chloride hydrogel-based flexible substrate to form an electrochromic layer on the surface of the 2-acrylamide-2-methylpropane sulfonic acid / acrylamide / acrylic acid / lithium chloride hydrogel-based flexible substrate; optionally, the electrochromic solution is drop-coated on the glass surface to obtain the electrochromic layer, and then attached to a 2-acrylamide-2-methylpropane sulfonic acid / acrylamide / acrylic acid / lithium chloride hydrogel-based flexible substrate, thereby transferring the electrochromic layer to the surface of the 2-acrylamide-2-methylpropane sulfonic acid / acrylamide / acrylic acid / lithium chloride hydrogel-based flexible substrate; preferably, the conditions for the glass plasma hydrophilic treatment are: pressure 60 Pa, time 10 min, power 100 W; the drop-coated solution volume is 100 ul, the oven drying temperature is 60 ° C, and the oven drying time is 30 min; (7) A flexible acrylamide hydrogel substrate having a conductive electrode layer is attached to a flexible 2-acrylamide-2-methylpropane sulfonic acid / acrylamide / acrylic acid / lithium chloride hydrogel substrate having an electrochromic layer to prepare a flexible stretchable electrochromic device.

[0006] In the present invention, in step (1), acrylamide, acrylic acid, 2-acrylamide-2-methylpropane sulfonic acid, lithium chloride, ammonium persulfate, N,N-methylenebisacrylamide, polyvinyl pyrrolidone and deionized water are mixed to form a uniform solution, and then dried to obtain a 2-acrylamide-2-methylpropane sulfonic acid / acrylamide / acrylic acid / lithium chloride hydrogel-based flexible substrate. Preferably, the mass ratio of acrylamide, acrylic acid, 2-acrylamide-2-methylpropane sulfonic acid, lithium chloride, ammonium persulfate, N,N-methylenebisacrylamide, polyvinyl pyrrolidone and deionized water is (20-30): (10-17): (4-7): (10-20): (0.15-0.2): (0.1-0.15): (1.5-2): 100.

[0007] In the present invention, in step (2), acrylamide, ammonium persulfate, N,N-methylenebisacrylamide, polyvinyl pyrrolidone and deionized water are mixed and stirred, and then dried to obtain an acrylamide hydrogel-based flexible substrate. Preferably, the mass ratio of acrylamide, ammonium persulfate, N,N-methylenebisacrylamide, polyvinyl pyrrolidone and deionized water is (20-30): (0.15-0.2): (0.1-0.15): (1.5-2): 100.

[0008] In the present invention, in step (3), ethylene glycol and isopropanol constitute a co-mixing solvent; the co-mixing solvent is mixed with a poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid) solution and a surfactant to form a poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid / co-mixing solvent composite solution; the co-mixing solvent is mixed with silver nanowires to form a silver nanowire / co-mixing solvent composite solution; the poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid / co-mixing solvent composite solution and the silver nanowire / co-mixing solvent composite solution are mixed to form a silver nanowire / poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid composite solution. Preferably, the mass ratio of ethylene glycol to isopropanol is 1: (0.8-1.2); in the poly (3,4-ethylenedioxythiophene-polystyrene sulfonic acid) / co-mixing solvent composite solution, the mass ratio of the co-mixing solvent to the poly (3,4-ethylenedioxythiophene-polystyrene sulfonic acid) solution is 1: (3-5); in the silver nanowire / co-mixing solvent composite solution, the mass ratio of the co-mixing solvent to the silver nanowire is 1: (3-5); the mass ratio of the poly (3,4-ethylenedioxythiophene-polystyrene sulfonic acid) / co-mixing solvent composite solution to the silver nanowire / co-mixing solvent composite solution is (1.5-2.5): 1. The stirring time for mixing the co-mixing solvent, poly (3,4-ethylenedioxythiophene-polystyrene sulfonic acid) and the co-mixing solvent, and the mixing time for mixing the silver nanowire and the co-mixing solvent is 30 minutes. Preferably, by mass ratio, the ratio of the co-mixing solvent is ethylene glycol: isopropanol = 1:1, the co-mixing solvent: poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid solution = 1:4, the co-mixing solvent: silver nanowire = 1:4, and poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid / co-mixing solvent solution: silver nanowire / co-mixing solvent solution = 2:1.

[0009] In the present invention, in step (4), the silver nanowire / poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid) composite solution is spin-coated to prepare a conductive electrode layer; the spin-coating process is: the spin-coating speed is 1000-3000 r / min, the spin-coating time is 50-70 s, and the attachment time is 5-15 min. Preferably, the spin-coating speed is 1000-3000 r / min, the spin-coating time is 60 s, and the hydrogel attachment time is 10 min.

[0010] In the present invention, in step (5), a one-step hydrothermal method is used to prepare tungsten oxide quantum dots, the temperature of the hydrothermal reaction is 170-190°C, and the time of the hydrothermal reaction is 40-55 hours. Preferably, the temperature of the hydrothermal reaction is 180°C, and the time of the hydrothermal reaction is 48 hours. In the tungsten oxide quantum dot / poly (3,4-ethylenedioxythiophene)-poly (styrene) sulfonic acid electrochromic solution, the concentration of poly (3,4-ethylenedioxythiophene)-poly (styrene) sulfonic acid in the poly (3,4-ethylenedioxythiophene)-poly (styrene) sulfonic acid solution is 1.3%; the mass ratio of the poly (3,4-ethylenedioxythiophene)-poly (styrene) sulfonic acid solution, the tungsten oxide quantum dot solution, and H2O is 1:2:1, and the surfactant content is 0.25%.

[0011] The present invention discloses the application of the flexible stretchable electrochromic device in preparing a flexible color-changing device or as a flexible color-changing device. Further, the present invention discloses the application of the flexible stretchable electrochromic device in preparing an intelligent soft electronic device.

[0012] The hydrogel-based flexible substrate of the flexible stretchable electrochromic device of the present invention is a 2-acrylamide-2-methylpropane sulfonic acid / acrylamide / acrylic acid / lithium chloride hydrogel-based flexible substrate and an acrylamide hydrogel-based flexible substrate; the electrochromic layer is prepared by drop coating of a tungsten oxide quantum dot / poly 3,4-ethylenedioxythiophene-polystyrene sulfonic acid composite solution; the conductive electrode layer is prepared by spin coating of a silver nanowire / poly 3,4-ethylenedioxythiophene-polystyrene sulfonic acid composite solution. The acrylamide hydrogel flexible substrate with the conductive electrode layer transferred is attached to the 2-acrylamide-2-methylpropane sulfonic acid / acrylamide / acrylic acid / lithium chloride hydrogel flexible substrate with the electrochromic layer transferred to prepare a flexible stretchable electrochromic device.

[0013] The thickness of the 2-acrylamide-2-methylpropane sulfonic acid / acrylamide / acrylic acid / lithium chloride hydrogel-based flexible substrate of the present invention is 2 to 5 mm; the thickness of the acrylamide hydrogel-based flexible substrate is 2 to 5 mm; the thickness of the electrochromic layer is 0.3 to 3 um; and the thickness of the conductive electrode layer is 1 to 3 mm. Preferably, the thickness of the 2-acrylamide-2-methylpropane sulfonic acid / acrylamide / acrylic acid / lithium chloride hydrogel-based flexible substrate of the present invention is 3 to 4 mm; the thickness of the acrylamide hydrogel-based flexible substrate is 3 to 4 mm; the thickness of the electrochromic layer is 0.357 to 2.56 um; and the thickness of the conductive electrode layer is 1 to 2 mm.

[0014] Beneficial effects of the present invention: (1) The present invention prepares an electrochromic composite solution by mixing tungsten oxide quantum dots prepared by a hydrothermal method with a poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid solution, which exhibits excellent response speed and good optical contrast. The color-changing properties of the electrochromic solution are regulated by adjusting the mass ratio of tungsten oxide quantum dots to the poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid solution. The preparation process is simple, safe and reliable.

[0015] (2) The flexible electrochromic device prepared by the present invention uses hydrogel to replace traditional flexible materials (polyester, polydimethylsiloxane, polyimide, etc.) as the flexible substrate, which solves the defects of existing flexible electrochromic devices such as poor flexibility, poor stretching cycle stability, and complex assembly, and broadens its application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] In order to more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the following briefly introduces the drawings required for use in the embodiments or the prior art description: Figure 1 This is a flow chart for the preparation of flexible electrochromic devices.

[0017] Figure 2 These are the transmittance and stress-strain curves of acrylamide hydrogel and 2-acrylamido-2-methylpropane sulfonic acid / acrylamide / acrylic acid / lithium chloride hydrogel.

[0018] Figure 3 is the square resistance of the conductive electrode layer prepared at different spin coating speeds.

[0019] Figure 4 It is the transmittance curve of the conductive electrode layer prepared at different spin coating speeds.

[0020] Figure 5 This is the transmission electron microscope image of tungsten oxide quantum dots and the particle size distribution diagram.

[0021] Figure 6 It is the transmittance curve of drop-coated tungsten oxide quantum dots / poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid) electrochromic composite solution with different volumes.

[0022] Figure 7 It is a scanning electron microscope cross-sectional image of the electrochromic layer prepared by drop coating different volumes of tungsten oxide quantum dots / poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid electrochromic composite solution.

[0023] Figure 8 This is a transmittance diagram of the flexible electrochromic device prepared by drop-coating different volumes of electrochromic solution before and after electrochromism.

[0024] Fig. 9 The invention discloses the cyclic stretching performance of the 2-acrylamide-2-methylpropane sulfonic acid / acrylamide / acrylic acid / lithium chloride hydrogel for transferring the electrochromic layer in Example 1 and the electrochromic performance after cyclic stretching.

[0025] Fig.10 This is a scanning electron microscope plan view of the 2-acrylamide-2-methylpropanesulfonic acid / acrylamide / acrylic acid / lithium chloride hydrogel before and after cyclic stretching of the electrochromic layer transferred in Example 1.

[0026] Fig.11 This is an optical picture of the working electrode composite photochromic hydrogel electrolyte layer after stretching.

[0027] Fig.12 It is the stress-strain curve of the working electrode composite photochromic hydrogel electrolyte layer with the existing electrochromic layer transferred. DETAILED DESCRIPTION

[0028] In the prior art, silver nanowires are easily oxidized in a long-term electrochemical cycle environment or a humid environment, resulting in a rapid deterioration in the performance of electrodes with silver nanowire networks, and the substrate often needs to be modified; the embedded structure, coating structure and protective layer structure designed in the present invention can improve the stability of silver nanowires; the hydrogel composed of hydrophilic polymers has excellent chemical biocompatibility and mechanical biocompatibility, enabling it to match well with soft tissues and exhibit excellent mechanical compliance. At the same time, the hydrogel exhibits excellent conductivity, adhesion and stretchability, which plays a vital role in flexible electronics.

[0029] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. In the description of the present invention, the reference to "embodiment", "one embodiment" or "other embodiments" indicates that the specific features, structures or characteristics described in conjunction with the embodiments include at least some embodiments, but not necessarily all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. The raw materials used in the present invention are all existing products, and the specific preparation operations and performance tests are conventional techniques.

[0030] The acrylic acid contained in the 2-acrylamide-2-methylpropane sulfonic acid / acrylamide / acrylic acid / lithium chloride hydrogel can induce the crystalline nanofiber structure of the poly (3,4-ethylenedioxythiophene) chain in the tungsten oxide quantum dot / poly (3,4-ethylenedioxythiophene)-poly (styrene sulfonic acid) composite electrochromic layer, thereby isolating the positively charged poly (3,4-ethylenedioxythiophene) and the negatively charged poly (styrene sulfonic acid), and improving the stretchability of the electrochromic layer. At the same time, based on the excellent flexibility and transparency of the hydrogel-based flexible substrate itself, the overall stretchability of the device is enhanced. Therefore, if Figure 1 As shown, the present invention constructs a multilayer composite structure through transfer technology to prepare a flexible and stretchable electrochromic device, which shows broad application prospects in the fields of wearable devices, stretchable and portable display electronic products, etc.

[0031] The raw materials and molds used in the present invention are existing products, and the specific preparation operations and performance tests are conventional technologies, wherein the poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid solution is a PH1000 reagent produced by Heraeus Electronic Materials. Mechanical property test: The tensile performance test of the device is carried out using a Mark-10 seriesf mesur mechanical testing machine. Conductive electrode square resistance test: The conductive electrode is tested for square resistance using an ST-2258C digital four-probe. Transmittance and optical contrast test: An ultraviolet spectrophotometer is used to measure the transmittance of the conductive electrode and the electrochromic layer, as well as the transmittance difference of the device in the colored and faded states at a wavelength of 550nm. Example 1

[0032] A method for preparing a flexible and stretchable electrochromic device, comprising the following steps: (1) Preparation of 2-acrylamide-2-methylpropane sulfonic acid / acrylamide / acrylic acid / lithium chloride hydrogel: 5 g acrylamide, 2.8 g acrylic acid, 1.2 g 2-acrylamide-2-methylpropane sulfonic acid and 3 g lithium chloride were weighed into a beaker, 20 g deionized water was added, and the mixture was stirred for 30 min to form a uniform mixed solution; then 0.34 g polyvinyl pyrrolidone, 0.025 g N,N-methylenebisacrylamide and 0.036 g ammonium persulfate were added to the mixed solution, and the mixture was stirred for 30 min and then transferred to a conventional mold, placed in a 60 °C oven for 60 min, and then the temperature was raised to 80 °C, and the mixture was taken out after being kept warm for 30 min, and naturally cooled to room temperature to obtain 2-acrylamide-2-methylpropane sulfonic acid / acrylamide / acrylic acid / lithium chloride hydrogel; (2) Preparation of acrylamide hydrogel: Weigh 5g acrylamide into a beaker, add 20g deionized water, and stir on a stirring table for 30 minutes to form a uniform mixed solution. Then add 0.34g polyvinyl pyrrolidone, 0.025g N,N-methylenebisacrylamide and 0.036g ammonium persulfate to the mixed solution, continue stirring for 30 minutes, transfer to a mold, place in a 60℃ oven for 60 minutes, then increase the temperature to 80℃, continue to keep warm for 30 minutes, take out, and naturally cool to room temperature to obtain acrylamide hydrogel; (3) Preparation of silver nanowire / poly (3,4-ethylenedioxythiophene)-poly (styrene sulfonic acid) conductive solution: Ethylene glycol and isopropanol were prepared in a ratio of 1:1 to form a co-solvent; 0.4 g of the co-solvent, 1.6 g of poly (3,4-ethylenedioxythiophene)-poly (styrene sulfonic acid) solution and 0.025 g of Triton-X100 solution were weighed into a beaker and stirred for 30 min to form a poly (3,4-ethylenedioxythiophene)-poly (styrene sulfonic acid) / co-solvent composite solution; 1 g of silver nanowire ( Isopropanol solvent, diameter 50nm, concentration 20mg / mL) was mixed with 4g of co-mixing solvent, and stirred on a stirring table for 30min to form a silver nanowire / co-mixing solvent composite solution; 2g of poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid / co-mixing solvent composite solution and 1g of silver nanowire / co-mixing solvent composite solution were mixed, and stirred for 30min to prepare a silver nanowire / poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid composite solution without flocculent precipitation; (4) Preparation of tungsten oxide quantum dots: 8.25 g of sodium tungstate dihydrate was dissolved in 25 g of deionized water solution. After complete dissolution, concentrated hydrochloric acid (37%) solution was added to form a white precipitate. The mixture was then centrifuged at 8000 r / min for 5 min. The supernatant solution was removed and the precipitate was washed with deionized water. This operation was repeated until the pH of the precipitate was neutral. The precipitate was then mixed with 25 mL of ethylene glycol and stirred at 90°C to form a transparent colorless solution. The solution was transferred to a 100 mL polytetrafluoroethylene reactor and heated in an oven at 180°C for 48 h, and then cooled to room temperature. The resulting solution was placed in a 1000 molecular weight dialysis bag for 24 h to remove impurities in the solution. The solution was taken out to obtain a tungsten oxide quantum dot solution. (5) Preparation of tungsten oxide quantum dots / poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid) composite electrochromic solution: Weigh 1 g of poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid solution, 2 g of tungsten oxide quantum dots solution and 0.025 g of Triton-X100 solution, add them into 1 g of deionized water to prepare a mixed solution, and stir continuously for 24 h to prepare a tungsten oxide quantum dots / poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid) composite electrochromic solution; (6) Preparation of electrochromic layer: First, the glass sheet is placed in ethanol and deionized water solution for ultrasonic cleaning for 10 minutes, and then placed in an oven to dry. After that, the cleaned glass sheet is placed in a plasma cleaning machine and plasma cleaned for 10 minutes at a working power of 120W and a working pressure of 300Pa to improve the hydrophilicity of the glass surface. Then, 100ul of tungsten oxide quantum dots / poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid composite solution is drop-coated on the hydrophilic treated glass surface, dried in an oven at 60°C for 30 minutes, and taken out to make an electrochromic layer; (7) Preparation of a conductive electrode layer: The glass sheet was cleaned according to the above steps, and then the silver nanowire / poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid) composite solution was spin-coated on the glass surface at a speed of 2000 r / min for 60 s. The spin-coated glass was transferred to a 60°C oven and dried for 30 min to form a conductive electrode layer. (8) Preparation of electrochromic layer / 2-acrylamide-2-methylpropane sulfonic acid / acrylamide / acrylic acid / lithium chloride hydrogel: The prepared electrochromic layer is transferred to the hydrogel surface by transfer printing. The specific method is as follows: First, the electrochromic solution is dropped on the glass surface and dried in a 60°C oven for 30 minutes to form an electrochromic layer; then, the prepared 2-acrylamide-2-methylpropane sulfonic acid / acrylamide / acrylic acid / lithium chloride hydrogel is placed on the glass surface with the electrochromic layer, and pressed for 1 minute to make the hydrogel surface in close contact with the electrochromic layer, and then left to stand at room temperature for 10 minutes to transfer the electrochromic layer to the hydrogel surface; (9) Preparation of conductive electrode layer / acrylamide hydrogel: referring to the method of step (8), transferring the conductive electrode to the surface of the acrylamide hydrogel; (10) Preparation of flexible electrochromic devices: The electrochromic layer / 2-acrylamide-2-methylpropane sulfonic acid / acrylamide / acrylic acid / lithium chloride hydrogel and the conductive electrode layer / acrylamide hydrogel were composited, and the electrochromic layer and the conductive electrode layer were brought into close contact by conventional pressing for 2 min to prepare a flexible electrochromic device, wherein the thickness of the 2-acrylamide-2-methylpropane sulfonic acid / acrylamide / acrylic acid / lithium chloride hydrogel-based flexible substrate and the acrylamide hydrogel-based flexible substrate were both 3 mm; the thickness of the conductive electrode layer was 1 mm.

[0033] Figure 2 The permeability and stress-strain curves of acrylamide hydrogel and 2-acrylamido-2-methylpropane sulfonic acid / acrylamide / acrylic acid / lithium chloride hydrogel; Figure 2 It can be seen that the transmittances of the 2-acrylamido-2-methylpropanesulfonic acid / acrylamide / acrylic acid / lithium chloride hydrogel and acrylamide hydrogel prepared above at 550nm are 91.4% and 88.3%, respectively; the tensile breaking strengths are 92KPa and 87KPa, respectively, and the tensile breaking elongations are 450% and 280%, respectively.

[0034] As can be seen from Table 1, the prepared devices have excellent properties such as tensile elongation, tensile cycle stability, and optical contrast after coloring and fading, which are comparable to most of the properties reported in the literature, indicating that they have excellent flexible stretchability and tensile cycle stability. Example 2

[0035] On the basis of Example 1, the drop coating amount of the tungsten oxide quantum dots / poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid composite solution in step (6) was changed to 50ul, and the spin coating speed in step (7) was changed to 1000r / min. The rest were the same, and conductive electrode layers prepared at different spin coating speeds were obtained. The rest were the same, and a flexible and stretchable electrochromic device was obtained. Example 3

[0036] On the basis of Example 1, the drop coating amount of the tungsten oxide quantum dots / poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid composite solution in step (6) was changed to 200ul, and the spin coating speed in step (7) was changed to 3000r / min. The rest were the same, and conductive electrode layers prepared at different spin coating speeds were obtained. The rest were the same, and a flexible and stretchable electrochromic device was obtained.

[0037] Figure 3 is the square resistance of the conductive electrode layer prepared at different spin coating speeds; Figure 4 It is the transmittance curve of the conductive electrode layer prepared at different spin coating speeds. It can be seen that the square resistance of the conductive electrode layer prepared at a spin coating speed of 2000r / min is 246Ω / sq, and the transmittance is 78%; the square resistance of the conductive electrode layer prepared at a spin coating speed of 1000r / min is 144Ω / sq, and the transmittance is 68%; the square resistance of the conductive electrode layer prepared at a spin coating speed of 3000r / min is 352Ω / sq, and the transmittance is 80%.

[0038] Figure 5 It is a transmission electron microscope image and a particle size distribution diagram of tungsten oxide quantum dots; it can be seen that the present invention successfully prepared tungsten oxide quantum dots using a hydrothermal method, and the prepared tungsten oxide quantum dots can be evenly distributed in an aqueous solution, and the average particle size is 3.14±0.55nm.

[0039] Figure 6 It is the transmittance curve of drop coating of different volumes of tungsten oxide quantum dots / poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid electrochromic composite solution; the electrochromic layer prepared by drop coating of 100ul electrochromic composite solution has a transmittance of 60%; the electrochromic layer prepared by drop coating of 50ul electrochromic composite solution has a transmittance of 70%; the electrochromic layer prepared by drop coating of 200ul electrochromic composite solution has a transmittance of 38%.

[0040] Figure 7This is a scanning electron microscope cross-sectional view of the electrochromic layer prepared by drop-coating different volumes of tungsten oxide quantum dots / poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid) electrochromic composite solution; the electrochromic layer prepared by drop-coating 100ul of the electrochromic composite solution has a thickness of 1.31um; the electrochromic layer prepared by drop-coating 50ul of the electrochromic composite solution has a thickness of 357nm; the electrochromic layer prepared by drop-coating 200ul of the electrochromic composite solution has a thickness of 2.56um.

[0041] Figure 8 The present invention is a transmittance diagram of a flexible electrochromic device prepared by drop-coating different volumes of electrochromic solution before and after electrochromism; the optical contrast of a flexible stretchable electrochromic device prepared by drop-coating 100ul of the electrochromic composite solution into an electrochromic layer is 34% (Example 1); the optical contrast of a flexible stretchable electrochromic device prepared by drop-coating 50ul of the electrochromic composite solution into an electrochromic layer is 15.7% (Example 2); the optical contrast of a flexible stretchable electrochromic device prepared by drop-coating 200ul of the electrochromic composite solution into an electrochromic layer is 14.8% (Example 3).

[0042] Fig. 9 The invention discloses a 2-acrylamide-2-methylpropane sulfonic acid / acrylamide / acrylic acid / lithium chloride hydrogel with transferred electrochromic layer and its electrochromic property after cyclic stretching. The prepared 2-acrylamide-2-methylpropane sulfonic acid / acrylamide / acrylic acid / lithium chloride hydrogel with transferred electrochromic layer can withstand 1000 cycles of cyclic stretching (200% tensile elongation) and can still maintain excellent electrochromic property after stretching.

[0043] Fig.10 The figure is a scanning electron microscope plan view of the 2-acrylamide-2-methylpropanesulfonic acid / acrylamide / acrylic acid / lithium chloride hydrogel transferred with an electrochromic layer before and after cyclic stretching. After 1000 stretching cycles (200% tensile elongation), the prepared 2-acrylamide-2-methylpropanesulfonic acid / acrylamide / acrylic acid / lithium chloride hydrogel transferred with an electrochromic layer has only small ripples on its microscopic surface, and no visible cracks appear, showing excellent cyclic stretching performance.

[0044] The present invention synthesizes a silver nanowire / poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid) conductive electrode with stable electrochemical performance and a highly transparent and stretchable hydrogel polymer. At the same time, tungsten oxide quantum dots were synthesized by a hydrothermal method, and an electrochromic material with fast response and excellent cycle stability was prepared by compounding it with a poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid solution. A high-performance flexible electrochromic device was prepared by constructing a multilayer composite structure. The device exhibits excellent response speed, cycle stability and optical contrast, and can achieve bending, twisting and excellent tensile properties at any angle. It has broad application prospects in wearable intelligent display and visual perception.

[0045] In the previously disclosed patent application (CN2023104346258, Example 1), the tensile elongation at break of the working electrode composite photochromic hydrogel electrolyte layer transferred with the electrochromic layer is 50%. After repeated stretching 5 times at a tensile elongation of 20%, visible cracks appear in the electrochromic layer, which will lead to a decrease in electrochromic performance. Fig.11 , Fig.12 . Compared with the previously published patents, the device prepared by the present invention exhibits excellent stretchability and stretch cycle stability, and can still maintain the integrity of the electrochromic layer after 1000 stretch cycles under the condition of 200% stretching elongation. In addition, it exhibits good optical contrast (DT=34%) and fast response speed. At the same time, adjustments and optimizations have been made in the synthesis process of the hydrogel flexible substrate and the conductive electrode layer, showing better transparency and conductivity.

[0046] Table 1 Comparison of stretchability and stretch cycle stability of Example 1 with related devices reported in the literature

[0047] In Table 1, the references corresponding to numbers 1-5 are as follows: [1] FAN Q, FAN H, LI K, et al. Stretchable, Electrochemically-StableElectrochromic Devices Based on Semi-Embedded Ag@Au Nanowire Network [J]. Small, 2023, 19(22): 2208234.

[0048] [2] WU W, POH WC, LV J, et al. Self-Powered and Light-Adaptable Stretchable Electrochromic Display [J]. Adv Energy Mater, 2023, 13(18):2204103.

[0049] [3] OH SJ, BAE J W. All-in-One plasticized Ionogel-based stretchable electrochromic devices [J]. Chem Eng J, 2023, 467: 143367.

[0050] [4] LINDERHED U, PETSAGKOURAKIS I, ERSMAN PA, et al. Fully screenprinted stretchable electrochromic displays [J]. Flexible and PrintedElectronics, 2021, 6(4): 045014.

[0051] [5] YUN TG, PARK M, KIM DH, et al. All-Transparent StretchableElectrochromic Supercapacitor Wearable Patch Device [J]. ACS Nano, 2019, 13(3): 3141-3150.

[0052] The above is based on the ideal embodiment of the present invention. Through the above description, relevant personnel can make various changes and modifications without departing from the technical concept of the present invention. The technical scope of the present invention is not limited to the content in the specification, and the technical scope must be determined according to the scope of the claims.

Claims

1. A method for preparing a flexible and stretchable electrochromic device, characterized in that: The following steps are involved: (1) Using acrylamide, acrylic acid, 2-acrylamide-2-methylpropane sulfonic acid and lithium chloride as raw materials, a 2-acrylamide-2-methylpropane sulfonic acid / acrylamide / acrylic acid / lithium chloride hydrogel-based flexible substrate was prepared; (2) Using acrylamide as raw material, preparing an acrylamide hydrogel-based flexible substrate; (3) using ethylene glycol, isopropanol, poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid) solution and silver nanowires as raw materials to form a silver nanowire / poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid composite solution; (4) preparing a silver nanowire / poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid) composite solution into a conductive electrode layer, and then attaching it to an acrylamide hydrogel flexible substrate to form a conductive electrode layer on the surface of the acrylamide hydrogel flexible substrate; (5) mixing tungsten oxide quantum dots with poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid) solution and surfactant to prepare tungsten oxide quantum dots / poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid electrochromic solution; (6) a tungsten oxide quantum dot / poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid electrochromic solution is prepared as an electrochromic layer, and then a 2-acrylamide-2-methylpropane sulfonic acid / acrylamide / acrylic acid / lithium chloride hydrogel-based flexible substrate is attached to form an electrochromic layer on the surface of the 2-acrylamide-2-methylpropane sulfonic acid / acrylamide / acrylic acid / lithium chloride hydrogel-based flexible substrate; (7) A flexible acrylamide hydrogel substrate having a conductive electrode layer is attached to a flexible 2-acrylamide-2-methylpropane sulfonic acid / acrylamide / acrylic acid / lithium chloride hydrogel substrate having an electrochromic layer to prepare a flexible stretchable electrochromic device.

2. The method for preparing a flexible and stretchable electrochromic device according to claim 1, characterized in that: In step (1), acrylamide, acrylic acid, 2-acrylamide-2-methylpropane sulfonic acid, lithium chloride, ammonium persulfate, N,N-methylenebisacrylamide, polyvinyl pyrrolidone and deionized water are mixed to form a uniform solution, which is then dried to obtain a 2-acrylamide-2-methylpropane sulfonic acid / acrylamide / acrylic acid / lithium chloride hydrogel-based flexible substrate.

3. The method for preparing a flexible and stretchable electrochromic device according to claim 1, characterized in that: In step (2), acrylamide, ammonium persulfate, N,N-methylenebisacrylamide, polyvinyl pyrrolidone and deionized water are mixed and stirred, and then dried to obtain an acrylamide hydrogel-based flexible substrate.

4. The method for preparing a flexible and stretchable electrochromic device according to claim 1, characterized in that: In step (3), ethylene glycol and isopropanol constitute a co-mixing solvent; the co-mixing solvent is mixed with a poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid) solution to form a poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid / co-mixing solvent composite solution; the co-mixing solvent is mixed with silver nanowires to form a silver nanowire / co-mixing solvent composite solution; the poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid / co-mixing solvent composite solution and the silver nanowire / co-mixing solvent composite solution are mixed to form a silver nanowire / poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid composite solution.

5. The method for preparing a flexible and stretchable electrochromic device according to claim 4, characterized in that: The mass ratio of ethylene glycol to isopropanol is 1:(0.8-1.2); in the composite solution of poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid / mixing solvent, the mass ratio of the mixing solvent to the poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid solution is 1:(3-5); in the composite solution of silver nanowires / mixing solvent, the mass ratio of the mixing solvent to the silver nanowires is 1:(3-5); the mass ratio of the composite solution of poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid / mixing solvent and the composite solution of silver nanowires / mixing solvent is (1.5-2.5):

1.

6. The method for preparing a flexible and stretchable electrochromic device according to claim 1, characterized in that: In step (4), the silver nanowire / poly (3,4-ethylenedioxythiophene)-polystyrene sulfonic acid) composite solution is spin-coated to prepare a conductive electrode layer; the spin-coating process is: spin-coating speed 1000-3000 r / min, spin-coating time 50-70 s; attachment time is 5-15 min.

7. The method for preparing a flexible and stretchable electrochromic device according to claim 1, characterized in that: In step (5), a one-step hydrothermal method is used to prepare a tungsten oxide quantum dot solution, the temperature of the hydrothermal reaction is 170-190° C., and the time of the hydrothermal reaction is 40-55 hours; in the tungsten oxide quantum dot / poly (3,4-ethylenedioxythiophene)-poly (styrene sulfonic acid) electrochromic solution, the mass ratio of poly (3,4-ethylenedioxythiophene)-poly (styrene sulfonic acid) solution, tungsten oxide quantum dot solution, and H2O is 1:2:1, and the surfactant content is 0.25%.

8. A flexible stretchable electrochromic device prepared according to the method for preparing a flexible stretchable electrochromic device according to claim 1.

9. Use of the flexible stretchable electrochromic device according to claim 8 in the preparation of a flexible color-changing device or as a flexible color-changing device.

10. Use of the flexible stretchable electrochromic device according to claim 8 in the preparation of intelligent soft electronic devices.

Citation Information

Patent Citations

  • Flexible electrochromic device and preparation method thereof

    CN110632803A

  • Tungstate quantum dot-based hydrogel color-changing device with electrochromism and photochromism and preparation method of tungstate quantum dot-based hydrogel color-changing device

    CN116540464A

  • Solar battery

    JP2016174151A

  • Single active layer electrochromic devices

    US20200192174A1

Cited By

  • Reflective electrochromic array structure and preparation method and application thereof

    CN122469553A