Silicon carbide ohmic contact structure, preparation method thereof and semiconductor device
By performing thermal oxygen growth repair on the doped region on the surface of the silicon carbide epitaxial layer and forming a multi-layer metal structure, the problems of rough surface and low contact quality of silicon carbide are solved, and a high-quality ohmic contact structure is achieved.
Patent Information
- Application Number
- CN202411166453.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-29
AI Technical Summary
There are difficulties in forming high-quality ohmic contact structures on the surface of silicon carbide semiconductor materials, which are often due to the problem of lowering the barrier height under the rough surface and the reverse voltage.
By performing thermal oxygen growth repair treatment on the doped region on the surface of the silicon carbide epitaxial layer, a silicon dioxide layer is formed and cleaned, and then a multi-layer metal structure is formed on the repaired surface, using the adhesion of the first metal layer and the second metal layer. Adhesion enhances adhesion, and optimizes the component ratio of the metal layer through materials such as nickel-aluminum alloy to improve contact effect.
The quality of ohmic contact is significantly improved, the problems of surface roughness and easy metal peeling are solved, and the contact effect between metal and semiconductor is improved.
Smart Images

Figure CN119049969A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the field of semiconductor technology, and in particular to a silicon carbide ohmic contact structure, a preparation method thereof, and a semiconductor device. Background Art
[0002] At present, the third generation of semiconductors represented by silicon carbide (SiC) and gallium nitride (GaN) are developing rapidly and have become an important branch of the semiconductor field. Unlike traditional silicon-based semiconductors, silicon carbide materials have a larger bandgap, a stronger critical electric field, and a higher electron migration rate, so more stable electronic devices with better characteristics can be manufactured. Currently, more and more traditional silicon-based semiconductor devices such as diodes, metal oxide semiconductor field effect transistors (MOSFETs), insulated gate bipolar transistors (IGBTs), etc. are being replaced by similar silicon carbide-based products.
[0003] In the manufacturing process of typical silicon carbide semiconductor devices, "metallization" is an essential process step. Processes such as chip bonding and interlayer interconnection are closely related to the metallization of the semiconductor surface. The metal deposited on the semiconductor surface often exists in two forms: "Schottky contact" and "ohmic contact". Ohmic contact is a non-rectifying contact. For example, Schottky diodes, MOSFETs and other devices contain a large number of ohmic contact areas.
[0004] In order to form ohmic contacts on the semiconductor surface, most existing solutions are to directly deposit specific metals on the semiconductor surface and then put it into a furnace for high-temperature sintering. However, due to the particularity of silicon carbide materials, the ohmic contact structure formed on its surface often has problems such as surface roughness caused by carbon precipitation or reduced barrier height under high reverse voltage. Therefore, how to form high-quality ohmic contacts on the surface of silicon carbide semiconductor substrates has become a difficult problem. Summary of the invention
[0005] The present invention provides a silicon carbide ohmic contact structure, a preparation method thereof and a semiconductor device to solve the problem of low quality of metal-semiconductor ohmic contact caused by surface roughness and other problems.
[0006] In a first aspect, the present disclosure provides a method for preparing a silicon carbide ohmic contact structure, comprising:
[0007] Doping a target area on the surface of the silicon carbide epitaxial layer to form a doped region on the surface of the silicon carbide epitaxial layer;
[0008] Performing a thermal oxygen growth repair process on the surface of the silicon carbide epitaxial layer where the doping region has been formed, so as to repair the rough surface of the silicon carbide epitaxial layer;
[0009] forming a metal layer on the repaired surface of the silicon carbide epitaxial layer;
[0010] The silicon carbide epitaxial layer on which the metal layer has been formed is subjected to high temperature sintering treatment to form an ohmic contact structure.
[0011] In some embodiments, performing a thermal oxygen growth repair process on the surface of the silicon carbide epitaxial layer where the doped region is formed includes:
[0012] Performing a thermal oxidation treatment on the surface of the silicon carbide epitaxial layer where the doped region is formed, so as to form a silicon dioxide layer on the surface of the silicon carbide epitaxial layer;
[0013] The surface of the silicon carbide epitaxial layer is cleaned with dilute hydrofluoric acid to remove the silicon dioxide layer formed on the surface of the silicon carbide epitaxial layer.
[0014] In some embodiments, the step of forming a metal layer on the repaired surface of the silicon carbide epitaxial layer comprises:
[0015] Generating a mask layer having a specified pattern on the repaired surface of the silicon carbide epitaxial layer;
[0016] forming a metal layer on the surface of the silicon carbide epitaxial layer on which the mask layer has been formed;
[0017] The mask layer and the metal layer on the mask layer are stripped off to leave a metal layer having a pattern structure consistent with a designated pattern on the surface of the silicon carbide epitaxial layer.
[0018] In some embodiments, the step of forming a metal layer on the repaired surface of the silicon carbide epitaxial layer comprises:
[0019] Depositing a first film layer material on the repaired surface of the silicon carbide epitaxial layer to form a first metal layer;
[0020] A second film layer material is deposited on the surface of the first metal layer to form a second metal layer.
[0021] The first metal layer has good adhesion, which is beneficial to the surface deposition of the second film layer material; the first metal layer can serve as a barrier layer to prevent the second metal layer from reacting with the silicon carbide epitaxial layer; the first metal layer itself can form a first ohmic contact with the semiconductor epitaxial layer, and when the second metal layer contacts the silicon carbide epitaxial layer over a large area, the path resistance can be reduced.
[0022] In some embodiments, the first film layer material includes titanium or titanium nitride;
[0023] The second film layer material includes any one of nickel-aluminum alloy, nickel, aluminum, molybdenum, and nickel-chromium alloy.
[0024] In some embodiments, the second film layer material is nickel-aluminum alloy;
[0025] When the doped region on the surface of the silicon carbide epitaxial layer is an N-type doped region, the proportion of nickel component in the nickel-aluminum alloy is 50% to 70%;
[0026] When the doped region on the surface of the silicon carbide epitaxial layer is a P-type doped region, the proportion of the aluminum component in the nickel-aluminum alloy is 70% to 80%.
[0027] Nickel and aluminum are high-quality ohmic contact metals, but nickel easily reacts with the silicon carbide epitaxial layer to form compounds, and aluminum has a low melting point and cannot withstand the sintering temperature of about 1000°C. By adjusting the reasonable metal ratio, the second metal layer can overcome the physical defects of metals such as nickel and aluminum in traditional solutions and enhance the robustness of the contact surface. Through the above improvements, the ohmic contact effect between metal and semiconductor can be significantly improved.
[0028] In some embodiments, when the doped region on the surface of the silicon carbide epitaxial layer is a low-concentration N-type doped region, the sintering temperature is 700-800° C.;
[0029] When the doped region on the surface of the silicon carbide epitaxial layer is a high-concentration N-type doped region, the sintering temperature is 850-950° C.;
[0030] When the doped region on the surface of the silicon carbide epitaxial layer is a P-type doped region, the sintering temperature is 900-1000°C.
[0031] In some embodiments, the thickness of the silicon dioxide layer is 50 nm to 150 nm; and the concentration of the hydrofluoric acid is 20%.
[0032] The thickness of the silicon dioxide layer generated by thermal oxidation treatment is controlled within 50nm to 150nm, and the concentration of hydrofluoric acid is controlled within 20%, so that a good repair effect can be achieved.
[0033] In a second aspect, the present disclosure provides a silicon carbide ohmic contact structure, including a silicon carbide ohmic contact structure prepared by the method for preparing the silicon carbide ohmic contact structure as described above.
[0034] In a third aspect, the present disclosure provides a semiconductor device comprising the silicon carbide ohmic contact structure as described above.
[0035] The present disclosure provides a silicon carbide ohmic contact structure, a preparation method thereof, and a semiconductor device, which have the following beneficial effects:
[0036] 1. Performing a thermal oxygen growth repair treatment on the surface of the silicon carbide epitaxial layer where the doped region has been formed to repair the rough surface of the silicon carbide epitaxial layer, thereby solving the surface roughness problem caused by carbon precipitation;
[0037] 2. By depositing the first metal layer and the second metal layer, the adhesion of the materials used between the two metal layers can be utilized to enhance the adhesion of the metal in the ohmic zone and solve the problem of easy metal peeling.
[0038] 3. If the second film layer material is nickel-aluminum alloy, the metal semiconductor contact effect can be improved by controlling the nickel content in the nickel-aluminum alloy to 50% to 70% in the N-type doping area and 70% to 80% in the P-type doping area according to the doping type of the doping area on the surface of the silicon carbide epitaxial layer.
[0039] 4. A good repair effect can be achieved by controlling the thickness of the silicon dioxide layer generated by thermal oxidation treatment within 50nm to 150nm and the hydrofluoric acid concentration within 20%. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] The present disclosure will be described in more detail below based on embodiments and with reference to the accompanying drawings:
[0041] Figure 1 A schematic diagram of a process for preparing a silicon carbide ohmic contact structure provided in an embodiment of the present disclosure;
[0042] Figure 2 A schematic diagram of forming a film layer structure provided in an embodiment of the present disclosure;
[0043] Figure 3 A schematic diagram of a process for preparing a silicon carbide ohmic contact structure provided in an embodiment of the present disclosure;
[0044] Figure 4 A schematic diagram of forming a film layer structure provided in an embodiment of the present disclosure;
[0045] Figure 5 A schematic diagram of a process for preparing a silicon carbide ohmic contact structure provided in an embodiment of the present disclosure;
[0046] Figure 6 A schematic diagram of forming a metal layer with a specified graphic structure provided in an embodiment of the present disclosure;
[0047] Figure 7 A schematic diagram of a process for preparing a silicon carbide ohmic contact structure provided in an embodiment of the present disclosure;
[0048] Figure 8 A schematic diagram of forming a metal layer of a specified graphic structure provided in an embodiment of the present disclosure.
[0049] In the drawings, the same reference numerals are used for the same components, and the drawings are not drawn to scale. DETAILED DESCRIPTION
[0050] In order to enable those skilled in the art to better understand the technical solution of the present disclosure, and to fully understand and implement how the present disclosure applies technical means to solve technical problems and achieve the corresponding technical effects, the technical solution in the embodiments of the present disclosure will be clearly and completely described below in conjunction with the drawings in the embodiments of the present disclosure. Obviously, the described embodiments are only embodiments of a part of the present disclosure, not all of the embodiments. The embodiments of the present disclosure and the various features in the embodiments can be combined with each other without conflict, and the technical solutions formed are all within the scope of protection of the present disclosure. Based on the embodiments in the present disclosure, all other embodiments obtained by ordinary technicians in this field without making creative work should fall within the scope of protection of the present disclosure.
[0051] It should be noted that the terms "first", "second", etc. in the specification and claims of the present disclosure and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchangeable where appropriate, so that the embodiments of the present disclosure described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product, or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products, or devices.
[0052] It should be noted that the steps shown in the flowcharts of the accompanying drawings can be executed in a computer system such as a set of computer executable instructions, and that, although a logical order is shown in the flowcharts, in some cases, the steps shown or described can be executed in an order different from that shown here.
[0053] In order to form ohmic contacts on the surface of semiconductors, most existing solutions directly deposit specific metals on the surface of semiconductors, and then put them into furnace tubes for high-temperature sintering. For example, typical ohmic contact metals such as nickel, aluminum, and tungsten are directly deposited on the surface of semiconductors, and then sintered at high temperature to form an ohmic contact structure. However, due to the particularity of silicon carbide materials, the ohmic contact structure formed on its surface often has problems such as surface roughness caused by carbon precipitation or reduced barrier height under large reverse voltage. Therefore, how to form high-quality ohmic contacts on the surface of silicon carbide semiconductor substrates has become a difficult problem.
[0054] Embodiment 1
[0055] Figure 1A schematic diagram of a process for preparing a silicon carbide ohmic contact structure provided in an embodiment of the present disclosure, Figure 2 Schematic diagram of the film structure provided in the embodiment of the present disclosure. Figure 1 and Figure 2 As shown, a method for preparing a silicon carbide ohmic contact structure comprises the following steps:
[0056] Step S11, doping a target area on the surface of the silicon carbide epitaxial layer to form a doped region on the surface of the silicon carbide epitaxial layer.
[0057] Specifically, the target area on the surface of the silicon carbide epitaxial layer is subjected to N-type doping or P-type doping by ion implantation or diffusion, wherein, if the target area on the surface of the silicon carbide epitaxial layer is subjected to P-type doping, the doped area on the surface of the silicon carbide epitaxial layer is a P-type doped area; if the target area on the surface of the silicon carbide epitaxial layer is subjected to N-type doping, the doped area on the surface of the silicon carbide epitaxial layer is an N-type doped area.
[0058] Step S12, performing a thermal oxygen growth repair treatment on the surface of the silicon carbide epitaxial layer where the doping region has been formed.
[0059] Since the silicon carbide epitaxial layer needs to be activated at high temperature to repair lattice damage and ensure impurity activity during impurity doping, the continuous high temperature process will cause carbon and silicon inside the silicon carbide to precipitate, resulting in a rough surface of the silicon carbide epitaxial layer. To address this problem, after the silicon carbide epitaxial layer is doped and formed, a thermal oxygen growth repair treatment is performed on the surface of the silicon carbide epitaxial layer to repair the rough surface of the silicon carbide epitaxial layer.
[0060] Specifically, step S12 includes the following steps:
[0061] Step S121, performing a thermal oxidation treatment on the surface of the silicon carbide epitaxial layer where the doping region is formed, so as to form a silicon dioxide layer on the surface of the silicon carbide epitaxial layer;
[0062] Step S122: Cleaning the surface of the silicon carbide epitaxial layer with dilute hydrofluoric acid to remove the silicon dioxide layer formed on the surface of the silicon carbide epitaxial layer.
[0063] The surface of the silicon carbide epitaxial layer is thermally oxidized by a furnace tube, and then the oxide layer on the surface of the silicon carbide epitaxial layer is removed by cleaning with low-concentration hydrofluoric acid. The cleaning process of hydrofluoric acid can be understood as the corrosion process of the semiconductor surface by strong acid, so it can also remove impurities such as metals, particles, organic contamination, etc. on the semiconductor surface.
[0064] Taking the silicon carbide epitaxial layer as an example, after high-temperature heat treatment at more than 1500°C, after doping the target area on the surface of the silicon carbide epitaxial layer, carbon precipitation occurs on the front side of the silicon carbide epitaxial layer, causing the surface of the formed silicon carbide epitaxial layer to be rough. At this time, the semiconductor surface is repaired by the above-mentioned thermal oxygen growth repair treatment method, and the average roughness Ra and root mean square roughness Rq of the surface of the silicon carbide epitaxial layer are measured by atomic force microscopy (AFM). Compared with before and after repair, the Ra value and Rq value are significantly reduced.
[0065] The test results show that a good repair effect can be achieved when the thickness of the silicon dioxide layer generated by thermal oxidation treatment is controlled within 50nm to 150nm and the hydrofluoric acid concentration is controlled within 20%. The hydrofluoric acid cleaning time should be adjusted according to the thickness of the silicon dioxide layer.
[0066] Step S13, forming a Figure 2 Specifically, the metal layer is made of an ohmic contact material, such as Ni, Al, etc.
[0067] Step S14, performing high temperature sintering on the silicon carbide epitaxial layer on which the metal layer has been formed to form an ohmic contact structure.
[0068] The method for preparing the silicon carbide ohmic contact structure provided in this embodiment performs a thermal oxygen growth repair treatment on the surface of the silicon carbide epitaxial layer where the doped region has been formed, so as to repair the rough surface of the silicon carbide epitaxial layer, thereby solving the surface roughness problem caused by carbon precipitation.
[0069] Embodiment 2
[0070] Figure 3 A schematic diagram of a process for preparing a silicon carbide ohmic contact structure provided in an embodiment of the present disclosure, Figure 4 Schematic diagram of the film structure provided in the embodiment of the present disclosure. Figure 3 and Figure 4 As shown, a method for preparing a silicon carbide ohmic contact structure comprises the following steps:
[0071] Step S21 , doping a target area on the surface of the silicon carbide epitaxial layer to form a doped region on the surface of the silicon carbide epitaxial layer.
[0072] Specifically, the target area on the surface of the silicon carbide epitaxial layer is subjected to N-type doping or P-type doping by ion implantation or diffusion, wherein, if the target area on the surface of the silicon carbide epitaxial layer is subjected to P-type doping, the doped area on the surface of the silicon carbide epitaxial layer is a P-type doped area; if the target area on the surface of the silicon carbide epitaxial layer is subjected to N-type doping, the doped area on the surface of the silicon carbide epitaxial layer is an N-type doped area.
[0073] Step S22, performing a thermal oxygen growth repair process on the surface of the silicon carbide epitaxial layer where the doping region has been formed.
[0074] Since the surface of the silicon carbide epitaxial layer needs to be activated at high temperature to repair lattice damage and ensure impurity activity when doping with impurities, and the continuous high temperature process will cause carbon and silicon inside the silicon carbide to precipitate, resulting in a rough surface of the silicon carbide epitaxial layer. To address this problem, after the silicon carbide epitaxial layer is doped and formed, the surface of the silicon carbide epitaxial layer is subjected to a thermal oxygen growth repair treatment to repair the rough surface of the silicon carbide epitaxial layer.
[0075] Specifically, step S22 includes the following steps:
[0076] Step S221, performing a thermal oxidation treatment on the surface of the silicon carbide epitaxial layer where the doping region is formed, so as to form a silicon dioxide layer on the surface of the silicon carbide epitaxial layer;
[0077] Step S222: Clean the surface of the silicon carbide epitaxial layer with dilute hydrofluoric acid to remove the silicon dioxide layer formed on the surface of the silicon carbide epitaxial layer.
[0078] The surface of the silicon carbide epitaxial layer is thermally oxidized by a furnace tube, and then the oxide layer on the surface of the silicon carbide epitaxial layer is removed by cleaning with low-concentration hydrofluoric acid. The cleaning process of hydrofluoric acid can be understood as the corrosion process of the semiconductor surface by strong acid, so it can also remove impurities such as metals, particles, organic contamination, etc. on the semiconductor surface.
[0079] Taking the silicon carbide epitaxial layer as an example, after high-temperature heat treatment at more than 1500°C, after doping the target area on the surface of the silicon carbide epitaxial layer, carbon precipitation occurs on the front side of the silicon carbide epitaxial layer, causing the surface of the formed silicon carbide epitaxial layer to be rough. At this time, the semiconductor surface is repaired by the above-mentioned thermal oxygen growth repair treatment method, and the surface average roughness Ra and root mean square roughness Rq of the silicon carbide epitaxial layer are measured using an atomic force microscope (AFM). Compared with before and after repair, the Ra value and Rq value have decreased significantly.
[0080] The test results show that a good repair effect can be achieved when the thickness of the silicon dioxide layer generated by thermal oxidation treatment is controlled within 50nm to 150nm and the hydrofluoric acid concentration is controlled within 20%. The hydrofluoric acid cleaning time should be adjusted according to the thickness of the silicon dioxide layer.
[0081] Step S23, depositing a first film material on the repaired surface of the silicon carbide epitaxial layer to form Figure 4 The first metal layer shown in .
[0082] Specifically, the first film layer material is deposited on the surface of the silicon carbide epitaxial layer by a PVD (physical vapor deposition) process. The first film layer material needs to be selected to have a barrier height suitable for being used as a metal that forms an ohmic contact with a semiconductor. For example, the first film layer material can be titanium (Ti), titanium nitride (TiN), or other metals of the same type.
[0083] The presence of the first metal layer has the following advantages:
[0084] (1) The first metal layer has good adhesion, which is conducive to the deposition of the second film layer material;
[0085] (2) The first metal layer can act as a barrier layer to prevent the second metal layer from reacting with the silicon carbide epitaxial layer;
[0086] (3) The first metal layer itself can form a first ohmic contact with the silicon carbide epitaxial layer. When the metal and the silicon carbide epitaxial layer are in contact with each other over a large area, the path resistance can be reduced.
[0087] In this embodiment, the first film layer material is metal Ti. Since metal Ti has good adhesion, stable characteristics, corrosion resistance, and does not react with oxygen and water at room temperature, its barrier height is also particularly suitable for forming an ohmic contact with a semiconductor. The excellent adhesion of metal Ti can effectively avoid metal peeling and improve the metal segregation phenomenon after high-temperature sintering.
[0088] Step S24, depositing a second film material on the surface of the first metal layer to form Figure 4 The second metal layer shown in FIG. The main function of the second metal layer is to fully form an ohmic contact in the semiconductor target area. In order to ensure a suitable ohmic contact roughness, the thickness of the second metal layer should be less than 300nm. If the thickness of the second metal layer is greater than 300nm, the ohmic contact roughness is too large, which affects the subsequent metal interconnection and packaging wire bonding.
[0089] Specifically, the second film layer material needs to select a barrier height suitable for being used as a metal that forms an ohmic contact with the semiconductor. For example, the second film layer material can be any one of nickel-aluminum alloy, nickel, aluminum, molybdenum, nickel-chromium alloy and other materials. In this embodiment, the second film layer material is nickel-aluminum alloy. Nickel-aluminum alloy, also known as "Leishman alloy", has a large number of metallic bonds and covalent bonds coexisting inside it, so that the material has the characteristics of high melting point, good thermal conductivity, oxidation resistance, corrosion resistance and the like. In the metallization process of the third-generation semiconductor, nickel and aluminum are two typical ohmic contact materials due to their high-quality material properties. By analyzing the material properties and combining the simulation results, it is found that: nickel and aluminum are combined to form an alloy, which is deposited on the surface of the semiconductor, and an ohmic layer metal can be formed under specific conditions. At the same time, the excellent properties of nickel-aluminum alloy itself can also improve the thickness control and metal stripping of nickel contact, while also avoiding the easy melting of aluminum at high temperatures, resulting in metal sintering.
[0090] The second metal layer is deposited on the surface of the first metal layer by magnetron sputtering, wherein the gas used for sputtering is argon. The metal target material components are set and deposited by a physical process. It is only necessary to ensure that the thickness and uniformity of the second metal layer meet the standards.
[0091] Specifically, the alloy composition is controlled by controlling the metal target composition to achieve a better metal-semiconductor contact effect. For example, the second film layer material is a nickel-aluminum alloy. When the doped region on the surface of the silicon carbide epitaxial layer is an N-type doped region, the nickel component in the nickel-aluminum alloy accounts for 50% to 70%; when the doped region on the surface of the silicon carbide epitaxial layer is a P-type doped region, the aluminum component in the nickel-aluminum alloy accounts for 70% to 80%.
[0092] Among them, when the doped region on the surface of the silicon carbide epitaxial layer is a low-concentration N-type doped region, the sintering temperature is 700-800°C; when the doped region on the surface of the silicon carbide epitaxial layer is a high-concentration N-type doped region, the sintering temperature is 850-950°C; when the doped region on the surface of the silicon carbide epitaxial layer is a P-type doped region, the sintering temperature is 900-1000°C.
[0093] Nickel and aluminum are both high-quality ohmic contact metals, but nickel easily reacts with the silicon carbide epitaxial layer to form compounds, and aluminum has a low melting point and cannot withstand a sintering temperature of around 1000°C. By adjusting the proportion of nickel and aluminum in the second metal layer according to the doping type and doping concentration of the silicon carbide epitaxial layer, the second metal layer can overcome the physical defects of metals such as nickel and aluminum in traditional solutions and enhance the robustness of the contact surface. Through the above improvements, the ohmic contact effect between metals and semiconductors can be significantly improved.
[0094] Step S25 , performing high temperature sintering on the silicon carbide epitaxial layer on which the first metal layer and the second metal layer have been formed to form an ohmic contact structure.
[0095] The ohmic contact structure prepared by the method for preparing the silicon carbide ohmic contact structure provided in this embodiment has the following advantages:
[0096] 1. Performing a thermal oxygen growth repair treatment on the surface of the silicon carbide epitaxial layer where the doped region has been formed to repair the rough surface of the silicon carbide epitaxial layer, thereby solving the surface roughness problem caused by carbon precipitation;
[0097] 2. By depositing the first metal layer and the second metal layer, the adhesion of the materials used between the two metal layers can be utilized to enhance the adhesion of the metal in the ohmic zone and solve the problem of easy metal peeling.
[0098] 3. If the second film layer material is nickel-aluminum alloy, the metal semiconductor contact effect can be improved by controlling the nickel content in the nickel-aluminum alloy to 50% to 70% for N-type silicon carbide epitaxial layer and 70% to 80% for P-type silicon carbide epitaxial layer according to the doping type of the silicon carbide epitaxial layer.
[0099] 4. A good repair effect can be achieved by controlling the thickness of the silicon dioxide layer generated by thermal oxidation treatment within 50nm to 150nm and the hydrofluoric acid concentration within 20%.
[0100] Embodiment 3
[0101] On the basis of the above embodiments, for the case where a metal layer of a specified structure needs to be formed, this embodiment provides a method for preparing a silicon carbide ohmic contact structure, such as Figure 5 As shown, this embodiment provides a method for preparing a silicon carbide ohmic contact structure, comprising:
[0102] Step S31 , doping a target area on the surface of the silicon carbide epitaxial layer to form a doped region on the surface of the silicon carbide epitaxial layer.
[0103] Specifically, the target area on the surface of the silicon carbide epitaxial layer is subjected to N-type doping or P-type doping by ion implantation or diffusion, wherein, if the target area on the surface of the silicon carbide epitaxial layer is subjected to P-type doping, the doped area on the surface of the silicon carbide epitaxial layer is a P-type doped area; if the target area on the surface of the silicon carbide epitaxial layer is subjected to N-type doping, the doped area on the surface of the silicon carbide epitaxial layer is an N-type doped area.
[0104] Step S32, performing a thermal oxygen growth repair process on the surface of the silicon carbide epitaxial layer where the doping region has been formed.
[0105] Since the silicon carbide epitaxial layer needs to be activated at high temperature to repair lattice damage and ensure impurity activity during impurity doping, the continuous high temperature process will cause carbon and silicon inside the silicon carbide to precipitate, resulting in a rough surface of the silicon carbide epitaxial layer. To address this problem, after the silicon carbide epitaxial layer is doped and formed, a thermal oxygen growth repair treatment is performed on the surface of the silicon carbide epitaxial layer to repair the rough surface of the silicon carbide epitaxial layer.
[0106] Specifically, step S32 includes the following steps:
[0107] Step S321, performing thermal oxidation treatment on the surface of the silicon carbide epitaxial layer where the doping region is formed, so as to form a silicon dioxide layer on the surface of the silicon carbide epitaxial layer;
[0108] Step S322: Clean the surface of the silicon carbide epitaxial layer with dilute hydrofluoric acid to remove the silicon dioxide layer formed on the surface of the silicon carbide epitaxial layer.
[0109] The surface of the silicon carbide epitaxial layer is thermally oxidized by a furnace tube, and then the oxide layer on the surface of the silicon carbide epitaxial layer is removed by cleaning with low-concentration hydrofluoric acid. The cleaning process of hydrofluoric acid can be understood as the corrosion process of the semiconductor surface by strong acid, so it can also remove impurities such as metals, particles, organic contamination, etc. on the semiconductor surface.
[0110] Taking the silicon carbide epitaxial layer as an example, after high-temperature heat treatment at more than 1500°C, after doping the target area on the surface of the silicon carbide epitaxial layer, carbon precipitation occurs on the front side of the silicon carbide epitaxial layer, causing the surface of the formed silicon carbide epitaxial layer to be rough. At this time, after the semiconductor surface is repaired by the above-mentioned repair treatment method, the surface average roughness Ra and root mean square roughness Rq of the silicon carbide epitaxial layer are measured using an atomic force microscope (AFM). Compared with before and after the repair, the Ra value and Rq value have decreased significantly.
[0111] The test results show that a good repair effect can be achieved when the thickness of the silicon dioxide layer generated by thermal oxidation treatment is controlled within 50nm to 150nm and the hydrofluoric acid concentration is controlled within 20%. The hydrofluoric acid cleaning time should be adjusted according to the thickness of the silicon dioxide layer.
[0112] Step S33, generating a Figure 6 The mask layer with a specified pattern is shown. Specifically, a mask with a specified pattern is formed on the surface of the silicon carbide epitaxial layer by using a photolithography process.
[0113] Step S34, forming a silicon carbide epitaxial layer on the surface of the silicon carbide epitaxial layer on which the mask layer has been generated. Figure 6 Specifically, the metal layer is made of an ohmic contact material, such as Ni, Al, etc.
[0114] Step S35, stripping the mask layer and the metal layer on the mask layer to leave a metal layer having a pattern structure consistent with the specified pattern on the surface of the silicon carbide epitaxial layer, such as Figure 6 Considering the resolution of the lift-off process, the thickness of the silicon carbide epitaxial layer is less than 100nm, with 50nm being optimal; the thickness of the metal layer is less than 300nm, with 150-200nm being optimal.
[0115] Specifically, step S33 and step S35 adopt a lift-off process. Figure 6 As shown, after the surface of the silicon carbide epitaxial layer is coated with photoresist, exposed, and developed to form a mask with a specified pattern, a metal layer is plated on the mask using a PVD process, and then a stripping solution (stripping solution) is used to dissolve the photoresist, remove the mask and strip the metal on the mask, so as to leave a metal layer with a graphic structure consistent with the specified pattern on the surface of the silicon carbide epitaxial layer, as shown in FIG. Figure 6 The metal structure shown in .
[0116] Step S36, performing high temperature sintering on the silicon carbide epitaxial layer on which the metal layer has been formed to form an ohmic contact structure.
[0117] The ohmic contact structure of the metal layer of the specified structure prepared by the method for preparing the silicon carbide ohmic contact structure provided in this embodiment has the following advantages:
[0118] 1. Performing a thermal oxygen growth repair treatment on the surface of the silicon carbide epitaxial layer where the doping region has been formed to repair the rough surface of the silicon carbide epitaxial layer, thereby solving the surface roughness problem caused by carbon precipitation;
[0119] 2. A good repair effect can be achieved by controlling the thickness of the silicon dioxide layer generated by thermal oxidation treatment within 50nm to 150nm and the hydrofluoric acid concentration within 20%.
[0120] Embodiment 4
[0121] On the basis of the above embodiments, for the case where a metal layer of a specified structure needs to be formed, this embodiment provides a method for preparing a silicon carbide ohmic contact structure, such as Figure 7 As shown, this embodiment provides a method for preparing a silicon carbide ohmic contact structure, comprising:
[0122] Step S41 , doping a target area on the surface of the silicon carbide epitaxial layer to form a doped region on the surface of the silicon carbide epitaxial layer.
[0123] Specifically, the target area on the surface of the silicon carbide epitaxial layer is subjected to N-type doping or P-type doping by ion implantation or diffusion, wherein, if the target area on the surface of the silicon carbide epitaxial layer is subjected to P-type doping, the doped area on the surface of the silicon carbide epitaxial layer is a P-type doped area; if the target area on the surface of the silicon carbide epitaxial layer is subjected to N-type doping, the doped area on the surface of the silicon carbide epitaxial layer is an N-type doped area.
[0124] Step S42, performing a thermal oxygen growth repair process on the surface of the silicon carbide epitaxial layer where the doping region has been formed.
[0125] Since the surface of the silicon carbide epitaxial layer needs to be activated at high temperature to repair lattice damage and ensure impurity activity when doping with impurities, and the continuous high temperature process will cause carbon and silicon inside the silicon carbide to precipitate, resulting in a rough surface of the silicon carbide epitaxial layer. To address this problem, after the silicon carbide epitaxial layer is doped and formed, the surface of the silicon carbide epitaxial layer is subjected to a thermal oxygen growth repair treatment to repair the rough surface of the silicon carbide epitaxial layer.
[0126] Specifically, step S42 includes the following steps:
[0127] Step S421, performing thermal oxidation treatment on the surface of the silicon carbide epitaxial layer where the doping region is formed, so as to form a silicon dioxide layer on the surface of the silicon carbide epitaxial layer;
[0128] Step S422: Clean the surface of the silicon carbide epitaxial layer with dilute hydrofluoric acid to remove the silicon dioxide layer formed on the surface of the silicon carbide epitaxial layer.
[0129] The surface of the silicon carbide epitaxial layer is thermally oxidized by a furnace tube, and then the oxide layer on the surface of the silicon carbide epitaxial layer is removed by cleaning with low-concentration hydrofluoric acid. The cleaning process of hydrofluoric acid can be understood as the corrosion process of the semiconductor surface by strong acid, so it can also remove impurities such as metals, particles, organic contamination, etc. on the semiconductor surface.
[0130] Taking the silicon carbide epitaxial layer as an example, after high-temperature heat treatment at more than 1500°C, after doping the target area on the surface of the silicon carbide epitaxial layer, carbon precipitation occurs on the front side of the silicon carbide epitaxial layer, causing the surface of the formed silicon carbide epitaxial layer to be rough. At this time, after the semiconductor surface is repaired by the above-mentioned repair treatment method, the surface average roughness Ra and root mean square roughness Rq of the silicon carbide epitaxial layer are measured using an atomic force microscope (AFM). Compared with before and after the repair, the Ra value and Rq value have decreased significantly.
[0131] The test results show that a good repair effect can be achieved when the thickness of the silicon dioxide layer generated by thermal oxidation treatment is controlled within 50nm to 150nm and the hydrofluoric acid concentration is controlled within 20%. The hydrofluoric acid cleaning time should be adjusted according to the thickness of the silicon dioxide layer.
[0132] Step S43, generating a Figure 8 The mask layer with a specified pattern is shown. Specifically, a mask with a specified pattern is formed on the surface of the silicon carbide epitaxial layer by using a photolithography process.
[0133] Step S44, depositing a first film material on the surface of the silicon carbide epitaxial layer on which the mask layer has been formed, to form Figure 8 The first metal layer shown in .
[0134] Specifically, the first film layer material is deposited on the surface of the silicon carbide epitaxial layer using a PVD process. The first film layer material needs to be selected to have a barrier height suitable for being used as a metal that forms an ohmic contact with a semiconductor. The first film layer material can be titanium (Ti), titanium nitride (TiN), or other metals of the same type. The presence of the first metal layer has the following advantages:
[0135] (1) The first metal layer has good adhesion, which is conducive to the surface deposition of the second film layer material;
[0136] (2) The first metal layer can act as a barrier layer to prevent the second metal layer from reacting with the silicon carbide epitaxial layer;
[0137] (3) The first metal layer itself can form a first ohmic contact with the semiconductor epitaxial layer. When the second metal layer contacts the silicon carbide epitaxial layer over a large area, the path resistance can be reduced.
[0138] In this embodiment, the first film layer material is metal Ti. Since metal Ti has good adhesion, stable characteristics, corrosion resistance, and does not react with oxygen and water at room temperature, its barrier height is also particularly suitable for forming an ohmic contact with a semiconductor. The excellent adhesion of metal Ti can effectively prevent metal peeling and improve the metal melting phenomenon after high-temperature sintering.
[0139] Step S45, depositing a second film material on the surface of the first metal layer to form Figure 8The second metal layer shown in . The main function of the second metal layer is to fully form an ohmic contact in the target area of the semiconductor. In order to ensure the appropriate ohmic contact roughness, the thickness of the second metal layer should be within 150nm to 300nm. If the thickness of the second metal layer is greater than 300nm, the ohmic contact roughness is too large, which affects the subsequent metal interconnection and packaging wire bonding. If the thickness of the second metal layer is less than 150nm, it is not conducive to the stripping process and is likely to cause the front metal to fall off.
[0140] Specifically, the second film layer material needs to select a barrier height suitable for being used as a metal that forms an ohmic contact with the semiconductor. The second film layer material can be any one of nickel-aluminum alloy, nickel, aluminum, molybdenum, and nickel-chromium alloy. In this embodiment, the second film layer material uses nickel-aluminum alloy. Nickel-aluminum alloy, also known as "Leishman alloy", has a large number of metallic bonds and covalent bonds coexisting inside it, so that the material has the characteristics of high melting point, good thermal conductivity, oxidation resistance, and corrosion resistance. In the metallization process of the third-generation semiconductor, nickel and aluminum are two typical ohmic contact materials due to their high-quality material properties. By analyzing the material properties and combining the simulation results, it is found that: nickel and aluminum are combined to form an alloy, which is deposited on the surface of the semiconductor, and an ohmic layer metal can be formed under specific conditions. At the same time, the excellent properties of nickel-aluminum alloy itself can also improve the thickness control and metal stripping of nickel contact, while also avoiding the problem that aluminum is easy to melt at high temperatures, leading to metal sintering.
[0141] The second metal layer is deposited on the surface of the first metal layer by magnetron sputtering, so the alloy composition can be controlled by controlling the metal target composition to achieve a better metal semiconductor contact effect. The gas used for sputtering is argon gas, the target composition is set, and deposition is carried out through a physical process. It is only necessary to ensure that the thickness and uniformity of the second metal layer meet the standards.
[0142] Specifically, the second film layer material is a nickel-aluminum alloy. When the doped region on the surface of the silicon carbide epitaxial layer is an N-type doped region, the nickel component in the nickel-aluminum alloy accounts for 50% to 70%; wherein, when the doped region on the surface of the silicon carbide epitaxial layer is a low-concentration N-type doped region, the sintering temperature is 700 to 800°C. When the doped region on the surface of the silicon carbide epitaxial layer is a high-concentration N-type doped region, the sintering temperature is 850 to 950°C.
[0143] When the doped region on the surface of the silicon carbide epitaxial layer is a P-type doped region, the proportion of aluminum components in the nickel-aluminum alloy is 70% to 80%, and the sintering temperature is 900 to 1000°C.
[0144] Nickel and aluminum are both high-quality ohmic contact metals, but nickel easily reacts with the silicon carbide epitaxial layer to form compounds, and aluminum has a low melting point and cannot withstand a sintering temperature of around 1000°C. By adjusting the proportion of nickel and aluminum in the second metal layer according to the doping type and doping concentration of the silicon carbide epitaxial layer, the second metal layer can overcome the physical defects of metals such as nickel and aluminum in traditional solutions and enhance the robustness of the contact surface. Through the above improvements, the ohmic contact effect between metals and semiconductors can be significantly improved.
[0145] Step S46, peeling off the mask layer, and the first metal layer and the second metal layer on the mask layer, leaving a metal layer having a pattern structure consistent with the specified pattern, such as Figure 8 Considering the resolution of the lift-off process, the thickness of the silicon carbide epitaxial layer is less than 100nm, with 50nm being optimal; the thickness of the first metal layer is less than 300nm, with 150-200nm being optimal; and the thickness of the second metal layer is 150nm-300nm.
[0146] Specifically, steps S43 to S46 adopt a lift-off process. Figure 8 As shown, after the surface of the silicon carbide epitaxial layer is coated with photoresist, exposed, and developed to form a mask with a specified pattern, a first metal layer and a second metal layer are sequentially plated on the mask using a PVD process, and then a stripping solution (stripping solution) is used to dissolve the photoresist, remove the mask, and strip the metal on the mask, leaving a pattern as shown on the surface of the silicon carbide epitaxial layer. Figure 8 The metal layer shown has a pattern structure consistent with the specified pattern, such as Figure 8 The metal structure shown in .
[0147] Step S47 , performing high temperature sintering on the silicon carbide epitaxial layer on which the first metal layer and the second metal layer have been formed to form an ohmic contact structure.
[0148] The ohmic contact structure of the metal layer of the specified structure prepared by the method for preparing the silicon carbide ohmic contact structure provided in this embodiment has the following advantages:
[0149] 1. Performing a thermal oxygen growth repair treatment on the surface of the silicon carbide epitaxial layer where the doped region has been formed to repair the rough surface of the silicon carbide epitaxial layer, thereby solving the surface roughness problem caused by carbon precipitation;
[0150] 2. By depositing the first metal layer and the second metal layer, the adhesion of the materials used between the two metal layers can be utilized to enhance the adhesion of the metal in the ohmic zone and solve the problem of easy metal peeling.
[0151] 3. If the second film layer material is nickel-aluminum alloy, the metal semiconductor contact effect can be improved by controlling the nickel content in the nickel-aluminum alloy to 50% to 70% in the N-type doping area and 70% to 80% in the P-type doping area according to the doping type of the doping area on the surface of the silicon carbide epitaxial layer.
[0152] 4. A good repair effect can be achieved by controlling the thickness of the silicon dioxide layer generated by thermal oxidation treatment within 50nm to 150nm and the hydrofluoric acid concentration within 20%.
[0153] Embodiment 5
[0154] Based on the above embodiments, this embodiment provides a silicon carbide ohmic contact structure, including a silicon carbide ohmic contact structure prepared by the method for preparing the silicon carbide ohmic contact structure as described in the above embodiments.
[0155] Embodiment 6
[0156] Based on the above embodiments, this embodiment provides a semiconductor device, including the silicon carbide ohmic contact structure as described in the above embodiments.
[0157] It should be noted that in the present disclosure, the terms "include", "comprises" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, an element limited by the sentence "includes a ..." does not exclude the existence of other identical elements in the process, method, article or device including the element.
[0158] Although the embodiments disclosed in the present disclosure are as above, the above contents are only embodiments adopted for facilitating the understanding of the present disclosure and are not intended to limit the present disclosure. Any technician in the technical field to which the present disclosure belongs can make any modifications and changes in the form and details of the implementation without departing from the spirit and scope disclosed in the present disclosure, but the scope of patent protection of the present disclosure shall still be subject to the scope defined in the attached claims.
Claims
1. A method for preparing a silicon carbide ohmic contact structure, characterized in that: include: Doping a target area on the surface of the silicon carbide epitaxial layer to form a doped region on the surface of the silicon carbide epitaxial layer; Performing a thermal oxygen growth repair process on the surface of the silicon carbide epitaxial layer where the doping region has been formed, so as to repair the rough surface of the silicon carbide epitaxial layer; forming a metal layer on the repaired surface of the silicon carbide epitaxial layer; The silicon carbide epitaxial layer on which the metal layer has been formed is subjected to high temperature sintering treatment to form an ohmic contact structure.
2. The preparation method according to claim 1, characterized in that: Performing a thermal oxygen growth repair process on the surface of the silicon carbide epitaxial layer where the doped region is formed, comprising: Performing a thermal oxidation treatment on the surface of the silicon carbide epitaxial layer where the doped region is formed, so as to form a silicon dioxide layer on the surface of the silicon carbide epitaxial layer; The surface of the silicon carbide epitaxial layer is cleaned with dilute hydrofluoric acid to remove the silicon dioxide layer formed on the surface of the silicon carbide epitaxial layer.
3. The preparation method according to claim 1, characterized in that: The step of forming a metal layer on the repaired surface of the silicon carbide epitaxial layer comprises: Generating a mask layer having a specified pattern on the repaired surface of the silicon carbide epitaxial layer; forming a metal layer on the surface of the silicon carbide epitaxial layer on which the mask layer has been formed; The mask layer and the metal layer on the mask layer are stripped off to leave a metal layer having a pattern structure consistent with a designated pattern on the surface of the silicon carbide epitaxial layer.
4. The preparation method according to any one of claims 1 to 3, characterized in that: The step of forming a metal layer on the repaired surface of the silicon carbide epitaxial layer comprises: Depositing a first film layer material on the repaired surface of the silicon carbide epitaxial layer to form a first metal layer; A second film layer material is deposited on the surface of the first metal layer to form a second metal layer.
5. The preparation method according to claim 4, characterized in that: The first film layer material includes titanium or titanium nitride; The second film layer material includes any one of nickel-aluminum alloy, nickel, aluminum, molybdenum, and nickel-chromium alloy.
6. The preparation method according to claim 5, characterized in that: The second film layer material is nickel-aluminum alloy; When the doped region on the surface of the silicon carbide epitaxial layer is an N-type doped region, the proportion of nickel component in the nickel-aluminum alloy is 50% to 70%; When the doped region on the surface of the silicon carbide epitaxial layer is a P-type doped region, the proportion of the aluminum component in the nickel-aluminum alloy is 70% to 80%.
7. The preparation method according to claim 6, characterized in that: When the doped region on the surface of the silicon carbide epitaxial layer is a low-concentration N-type doped region, the sintering temperature is 700-800° C.; When the doped region on the surface of the silicon carbide epitaxial layer is a high-concentration N-type doped region, the sintering temperature is 850-950° C.; When the doped region on the surface of the silicon carbide epitaxial layer is a P-type doped region, the sintering temperature is 900-1000°C.
8. The preparation method according to claim 2, characterized in that: The thickness of the silicon dioxide layer is 50nm-150nm; the concentration of the hydrofluoric acid is 20%.
9. A silicon carbide ohmic contact structure, characterized in that: It comprises a silicon carbide ohmic contact structure prepared by the method for preparing a silicon carbide ohmic contact structure according to any one of claims 1 to 8.
10. A semiconductor device, characterized in that: It comprises the silicon carbide ohmic contact structure as claimed in claim 9.