Preparation method of enhanced GaN HEMT device

Through electron beam activation of p-GaN cap layer and high-temperature annealing technology, the damage problem of traditional etching methods on GaN HEMT devices is solved, the performance and reliability of the device are improved, and the effects of high output current and low on-resistance are achieved.

CN119049971APending Publication Date: 2024-11-29XIDIAN UNIV +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411166944.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Traditional p-GaN dry etching method will cause etching damage and defects in the manufacturing of GaN HEMT devices, affecting the two-dimensional electronic air density and device performance, and high etching accuracy requirements. Improper depth will lead to reduced device saturation output current and Reduced reliability.

Method used

The p-GaN gate is prepared by electron beam selective activation of p-GaN cap layer, combining metal organic chemical vapor deposition and electron beam evaporation processes to reduce etching damage, and form ohmic contacts and Schottky contacts through high-temperature annealing to improve device performance .

Benefits of technology

It effectively reduces etching damage, improves the saturation current and reliability of the device, reduces dynamic on-resistance, achieves high output current and low on-resistance performance, and has high process compatibility and low material cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119049971A_ABST
    Figure CN119049971A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of an enhanced GaN HEMT device, and the method comprises the steps: sequentially growing a buffer layer, a channel layer, a barrier layer and a p-GaN cap layer on the surface of a substrate layer, obtaining an epitaxial structure, enabling the channel layer and the barrier layer to form a heterojunction, and enabling the channel layer and the barrier layer to form a two-dimensional electron gas as a conductive channel at the interface of the heterojunction; electron beam irradiation is carried out on part of the p-GaN cap layer, Mg impurities in the p-GaN cap layer are activated, and a P-type GaN gate is obtained; a gate metal electrode is prepared on the P-type GaN gate, and a two-dimensional electron gas conducting channel is regulated and controlled by the P-type GaN gate and the gate metal electrode; the p-type GaN gate is prepared by selectively activating the p-GaN cap layer through the electron beam, so that the influence of etching damage on the two-dimensional electron gas density and the dynamic characteristics of the device in the manufacturing process of a conventional enhanced GaN HEMT device is effectively reduced, the saturation current of the device is improved, the dynamic on-resistance of the device is reduced, and the reliability of the device is enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of semiconductor devices, and in particular to a method for preparing an enhanced GaN HEMT device. Background Art

[0002] New wide bandgap semiconductor materials represented by GaN have advantages such as large bandgap width, high electron mobility, high breakdown field strength, high saturation electron velocity and high thermal conductivity, making them a good choice for power semiconductor devices. GaN has excellent intrinsic material properties. In addition to the advantages shared by wide bandgap semiconductor materials, one of the biggest advantages of GaN is the existence of strong spontaneous polarization and piezoelectric polarization effects, which can form a high concentration of two-dimensional electron gas (2DEG) at the AlGaN / GaN interface to achieve conduction of the device channel.

[0003] Based on the strong spontaneous polarization and piezoelectric effect in GaN-based heterojunctions, conventional GaN HEMTs are depletion-mode devices, also known as normally-on devices. In practical applications, depletion-mode devices need to remain in the off state when driven by a negative voltage power supply, which not only poses a risk of circuit mis-opening, but also greatly increases circuit power consumption. Enhanced-mode GaN HEMTs are in the off state when the gate voltage is zero, that is, they do not require negative voltage drive when not in operation, which can greatly reduce additional power consumption and simplify the circuit.

[0004] The p-GaN cap layer technology enables enhanced GaN HEMT devices to eliminate the need for additional gate processing, and has the advantages of stable performance, high repeatability, and high reliability. It is the preferred technology for commercializing GaN power devices. However, the traditional p-GaN dry etching method will cause damage to the etched surface and introduce a large number of defects. At the same time, the p-GaN etching accuracy is also very critical. If the etching depth is too shallow or too deep, the two-dimensional electron gas below will be depleted, resulting in a decrease in the device's saturated output current, limiting device performance and reducing device reliability. Summary of the invention

[0005] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a method for preparing an enhancement-mode GaN HEMT device, in which a p-type GaN gate is prepared by selectively activating a p-GaN cap layer by an electron beam, which can effectively reduce the influence of etching damage generated in the manufacturing process of conventional enhancement-mode GaN HEMT devices on the two-dimensional electron gas density and the dynamic characteristics of the device, and is conducive to improving the saturation current of the device, reducing the dynamic on-resistance of the device, and enhancing the reliability of the device.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0007] A method for preparing an enhanced GaN HEMT device, characterized in that it comprises the following steps:

[0008] Step 1: using a metal organic chemical vapor deposition (MOCVD) process to sequentially grow a buffer layer 2, a channel layer 3, a barrier layer 4 and a p-GaN cap layer 5 on the surface of a substrate layer 1 to obtain an epitaxial structure;

[0009] Step 2: Photolithography is performed on the surface of the epitaxial structure in step 1 by using a photoresist reversal process to obtain a photoresist pattern in the gate region; then a layer of Au is further deposited on the surface of the epitaxial structure by an electron beam evaporation process, and a mask layer outside the gate region is obtained after peeling off;

[0010] Step 3: using an electron beam device to perform electron beam irradiation on the gate region of the epitaxial structure surface in step 2 that is not covered by the mask layer to activate the Mg impurities therein, and then cleaning the mask layer to obtain a p-type GaN gate 6;

[0011] Step 4: Photolithography is performed on the surface of the structure obtained in step 3 using a photoresist process to obtain a photoresist pattern in the mesa area; then etching is performed using a semiconductor material etcher (ICP), the etching depth starting from the p-GaN cap layer 5 until a portion of the channel layer 3 is etched away to form a mesa isolation;

[0012] Step 5: Photolithography is performed on the surface of the structure obtained in step 4 using a photoresist reversal process to obtain a photoresist pattern outside the source and drain electrode regions; then, a semiconductor material etcher (ICP) is used to perform etching to remove the p-GaN and AlGaN in the source and drain electrode regions; then, metal evaporation is performed using an electron beam evaporation process, and after stripping, a source electrode 7 and a drain electrode 8 are obtained;

[0013] Step 6: Perform rapid thermal annealing on the device obtained in step 5 in a N2 atmosphere, so that the source electrode 7 and the drain electrode 8 form an ohmic contact with the barrier layer 4;

[0014] Step 7: Photolithography is performed on the surface of the structure obtained in step 6 by using a photoresist reversal process to obtain a photoresist pattern other than the gate metal electrode; then metal evaporation is performed by using an electron beam evaporation process, and the gate metal electrode 9 is obtained after peeling; the gate metal electrode 9 forms a Schottky contact with the p-type GaN gate 6, and the two-dimensional electron gas in the lower channel layer 3 is depleted through the p-type GaN gate 6, and finally an enhanced GaN HEMT device is obtained.

[0015] In step 1, the material of the substrate layer 1 is Si, SiC, sapphire or diamond, with a thickness of 100-1500 μm; the material of the buffer layer 2 is AlN, GaN or AlGaN, with a thickness of 1000-6000 nm; the material of the channel layer 3 is GaN, AlGaN or InGaN, with a thickness of 200-1000 nm; the material of the barrier layer 4 is AlGaN, with a thickness of 10-25 nm, and the Al component is 0.05-0.25; the material of the p-GaN cap layer 5 is GaN, with a thickness of 50-140 nm, and the doping impurity is Mg, and the doping concentration is 5x10 17 – 5x10 20 cm -3 .

[0016] The epitaxial structure obtained in step 1 is immersed in a mixed solution of H2SO4 and H2O2 in a volume ratio of 7:3 to remove oxides and impurities on the surface of the epitaxial structure, and then organic cleaning is performed in acetone solution and isopropanol solution in sequence.

[0017] In step 4, the acceleration voltage of the electron beam is 10-50 kV, the emission current is 20-100 μA, and the beam size is 5-150 μm.

[0018] In the step 5, the structures of the source electrode 7 and the drain electrode 8 are Ti / Al / Ni / Au from bottom to top, and the thicknesses are 20 / 120 / 45 / 55 nm, respectively.

[0019] In step 6, the annealing temperature is 800-850° C., and the annealing time is 30-35 seconds.

[0020] In the step 7, the structures of the gate metal electrode 9 are Ni / Au from bottom to top, and the thicknesses are 30 / 120 nm.

[0021] After the photolithography operation in step 7, magnetron sputtering technology can be used to deposit W or TiN to obtain the gate metal electrode 9.

[0022] An enhanced GaN HEMT device is prepared by the above-mentioned preparation method.

[0023] Compared with the prior art, the beneficial effects of the present invention are:

[0024] The present invention prepares a p-type GaN gate by selectively activating a p-GaN cap layer by an electron beam, effectively reducing etching damage and avoiding a reduction in the density of a two-dimensional electron gas caused by etching, which is beneficial to improving the saturation current of the device, reducing gate leakage, and enhancing the reliability of the device; high-temperature annealing forms ohmic contact source-drain electrodes, and the adopted Schottky gate structure can achieve device performance of high output current and low on-resistance; the preparation method proposed by the present invention has high process compatibility, low material cost, and relatively simple process manufacturing steps. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a schematic diagram of the device structure formed after step 1 in the method for preparing an enhanced GaN HEMT device of the present invention.

[0026] Figure 2 It is a schematic diagram of the device structure formed after step 3 in the method for preparing the enhanced GaN HEMT device of the present invention.

[0027] Figure 3 It is a schematic diagram of the device structure formed after step 4 in the method for preparing the enhanced GaN HEMT device of the present invention.

[0028] Figure 4 It is a schematic diagram of the device structure formed after step 5 in the method for preparing the enhanced GaN HEMT device of the present invention.

[0029] Figure 5 It is a schematic diagram of the device structure formed after step 6 in the method for preparing the enhanced GaN HEMT device of the present invention.

[0030] Figure 6 It is a schematic diagram of the device structure formed after step 8 in the method for preparing an enhanced-mode GaN HEMT device of the present invention.

[0031] Figure 7 It is a top view of the structure of the enhancement mode GaN HEMT device of the present invention.

[0032] In the figure: 1-substrate layer; 2-composite buffer layer; 3-channel layer; 4-barrier layer; 5-p-GaN cap layer; 6-p-type GaN gate; 7-source electrode; 8-drain electrode; 9-gate metal electrode. DETAILED DESCRIPTION

[0033] The technical solution of the present invention is described in detail below in conjunction with the accompanying drawings and specific implementation methods.

[0034] like Figure 7As shown, an enhanced GaN HEMT device comprises a substrate layer 1, a buffer layer 2 and a channel layer 3 which are stacked in sequence from bottom to top; a barrier layer 4 and a source electrode 7 and a drain electrode 8 located on both sides of the barrier layer 4 are arranged on the channel layer 3; a p-type GaN gate 6 is arranged on the barrier layer 4, and a gate metal electrode 9 is arranged on the p-type GaN gate 6; the channel layer 3 and the barrier layer 4 form a heterojunction, and the interface of the heterojunction formed by the channel layer 3 and the barrier layer 4 forms a two-dimensional electron gas as a conductive channel; the source electrode 7 and the drain electrode 8 both form an ohmic contact with the two-dimensional electron gas, and the gate metal electrode 9 forms a Schottky contact with the p-GaN gate 6.

[0035] A method for preparing an enhanced GaN HEMT device comprises the following steps:

[0036] Step 1: A buffer layer 2, a channel layer 3, a barrier layer 4 and a p-GaN cap layer 5 are sequentially grown on the surface of a substrate layer 1 by using a metal organic chemical vapor deposition (MOCVD) process to obtain an epitaxial structure, such as Figure 1 As shown;

[0037] The substrate layer 1 is made of Si, SiC, sapphire or diamond with a thickness of 100-1500 μm. A buffer layer 2 with a thickness of 1000-6000 nm is grown on the substrate layer 1 at a low temperature of 500° C. The material of the buffer layer 2 is AlN, GaN or AlGaN. A channel layer 3 with a thickness of 200-1000 nm is grown on the buffer layer 2 at a temperature of 1000° C. The material of the channel layer 3 is GaN, AlGaN or InGaN. A barrier layer 4 with a thickness of 10-25 nm is epitaxially grown on the channel layer 3. The material of the barrier layer 4 is AlGaN with an Al component of 0.05-0.25. Finally, a p-GaN cap layer 5 with a thickness of 50-140 nm is epitaxially grown on the barrier layer 4. The material of the p-GaN cap layer 5 is GaN with an impurity doped with Mg and a doping concentration of 5×10 17 – 5x10 20 cm -3 ;

[0038] Step 2: Soak the epitaxial structure obtained in step 1 in a mixed solution of H2SO4 and H2O2 with a volume ratio of 7:3 for 1 minute to remove oxides and impurities on the surface of the epitaxial structure, and then perform organic cleaning in acetone solution and isopropanol solution for 5 minutes by ultrasonic treatment.

[0039] Step 3: Photolithography is performed on the surface of the epitaxial structure in step 1 using a photoresist reversal process to obtain a photoresist pattern in the gate region; then Au with a thickness of 5-10 nm is deposited on the surface of the epitaxial structure using an electron beam evaporation process at an evaporation rate of The vacuum degree is 5e-4Pa, and the mask layer outside the gate area is obtained after stripping, such as Figure 2 As shown;

[0040] Step 4: Use an electron beam device to perform electron beam irradiation on the gate area of ​​the epitaxial structure surface not covered by the mask layer in step 2 to activate the Mg impurities therein, and then clean the mask layer to obtain a p-type GaN gate 6, such as Figure 3 As shown; the acceleration voltage of the electron beam is 10-50 kV, the emission current is 20-100 μA, and the beam size is 5-150 μm;

[0041] Step 5: Photolithography is performed on the surface of the structure obtained in step 4 using a photoresist process to obtain a photoresist pattern in the mesa area; then etching is performed using a semiconductor material etcher (ICP), with the etching depth starting from the p-GaN cap layer 5 until a portion of the channel layer 3 is etched away to form a mesa isolation, such as Figure 4 As shown;

[0042] Step 6: Photolithography is performed on the surface of the structure obtained in step 5 by using a photoresist reversal process to obtain a photoresist pattern outside the source and drain electrode regions; then, a semiconductor material etcher (ICP) is used to perform etching to remove the p-GaN and AlGaN in the source and drain electrode regions; then, metal evaporation is performed by using an electron beam evaporation process, and source electrode 7 and drain electrode 8 are obtained after stripping. Figure 5 As shown; the structures of the source electrode 7 and the drain electrode 8 are Ti / Al / Ni / Au from bottom to top, and the thicknesses are 20 / 120 / 45 / 55nm, respectively, and the evaporation rate is The vacuum degree is 5e-4Pa;

[0043] Step 7: The device obtained in step 6 is rapidly thermally annealed in a N2 atmosphere at 800-850°C for 30-35s, so that the source electrode 7 and the drain electrode 8 form an ohmic contact with the barrier layer 4;

[0044] Step 8: Photolithography is performed on the surface of the structure obtained in step 7 by using a photoresist reversal process to obtain a photoresist pattern other than the gate metal electrode; then metal evaporation is performed by using an electron beam evaporation process, and a gate metal electrode 9 is obtained after peeling. The structure of the gate metal electrode 9 is Ni / Au from bottom to top, the thickness is 30 / 120nm, and the evaporation rate is The vacuum degree is 5e-4Pa; the gate metal electrode 9 forms a Schottky contact with the p-type GaN gate 6, and the two-dimensional electron gas in the lower channel layer 3 is depleted through the p-type GaN gate 6, and finally an enhanced GaN HEMT device is obtained, such as Figure 6 As shown;

[0045] The photoresist reversal process used in the above steps 3, 6 and 8 is as follows:

[0046] The photoresist is AZ5214 photoresist; the structure surface is coated with glue, the spinning speed is 4000r / min, and the spinning time is 30s; the structure after glue coating is pre-baked at 110°C for 1min using a hot plate; then an MA6 photolithography machine is used for exposure, and then reverse baking is performed, that is, maintaining at 120°C for 2min; then flood exposure is performed, and a photoresist pattern is obtained after development.

[0047] The photoresist process used in step 5 above is as follows:

[0048] The photoresist is AZ6112 photoresist; the structure surface is coated with the photoresist, the spinning speed is 4000r / min, and the spinning time is 35s; the epitaxial structure after the coating is pre-baked at 100°C for 1min using a hot plate; then an MA6 photolithography machine is used for exposure, and a photoresist pattern is obtained after development.

[0049] After the photolithography operation in the above step 8, W or TiN may be deposited by magnetron sputtering technology to obtain the gate metal electrode 9 .

[0050] Example 1

[0051] A method for preparing an enhanced GaN HEMT device comprises the following steps:

[0052] Step 1: using a metal organic chemical vapor deposition (MOCVD) process to sequentially grow a buffer layer 2, a channel layer 3, a barrier layer 4 and a p-GaN cap layer 5 on the surface of a substrate layer 1 to obtain an epitaxial structure;

[0053] First, a 3000nm thick GaN buffer layer 2 is grown on the substrate layer 1 at a low temperature of 500°C; a 200nm thick GaN channel layer 3 is grown on the GaN buffer layer 2 at a temperature of 1000°C, and a 15nm thick AlGaN barrier layer 4 is epitaxially grown on the GaN channel layer 3, with an Al composition of 0.21 and a Ga composition of 0.79; finally, a p-GaN cap layer 5 is epitaxially grown on the AlGaN barrier layer 4, with Mg doping and a doping concentration of 2.5×10 19 cm -3 , with a thickness of 90nm; the material of the substrate layer 1 is Si, with a thickness of 200μm;

[0054] Step 2: Soak the epitaxial structure obtained in step 1 in a mixed solution of H2SO4 and H2O2 with a volume ratio of 7:3 for 1 minute to remove oxides and impurities on the surface of the epitaxial structure, and then perform organic cleaning in acetone solution and isopropanol solution for 5 minutes by ultrasonic treatment.

[0055] Step 3: Photolithography is performed on the surface of the epitaxial structure cleaned in step 2 by using a photoresist reversal process to obtain a photoresist pattern in the gate region; then a layer of Au is further deposited on the surface of the epitaxial structure by an electron beam evaporation process, and a mask layer outside the gate region is obtained after peeling off;

[0056] Step 4: using an electron beam device to irradiate the gate region on the surface of the epitaxial structure in step 3 that is not covered by the mask layer, to activate the Mg impurities therein, and then cleaning the mask layer to obtain the p-type GaN gate 6; the acceleration voltage of the electron beam is 20 kV, the emission current is 60 μA, and the beam size is 10 μm;

[0057] Step 5: Use a photoresist process to perform photolithography on the surface of the structure obtained in step 4 to obtain a photoresist pattern in the mesa area; use a semiconductor material etcher ICP to perform etching with an etching depth of 200nm to form a mesa isolation, such as Figure 4 As shown;

[0058] Step 6: Photolithography is performed on the surface of the structure obtained in step 5 by using a photoresist reversal process to obtain a photoresist pattern outside the source and drain electrode regions; then, a semiconductor material etcher (ICP) is used for etching to remove the p-GaN in the source and drain electrode regions; then, Ti, Al, Ni, and Au are grown in sequence by an electron beam evaporation process, wherein the thickness of Ti is 20 nm, the thickness of Al is 120 nm, the thickness of Ni is 45 nm, and the thickness of Au is 55 nm, and source electrode 7 and drain electrode 8 are formed after peeling;

[0059] Step 7: The device obtained in step 6 is subjected to rapid thermal annealing for 32 seconds in a N2 atmosphere at 820°C, so that the source electrode 7 and the drain electrode 8 form ohmic contact with the barrier layer 4;

[0060] Step 8: Photolithography is performed on the surface of the structure obtained in step 7 by using a photoresist reversal process to obtain a photoresist pattern outside the gate metal electrode area; then Ni and Au are grown in sequence by an electron beam evaporation process, wherein the thickness of Ni is 30 nm and the thickness of Au is 120 nm, and a gate metal electrode 9 is obtained after peeling; the gate metal electrode 9 forms a Schottky contact with the p-type GaN gate 6, and the two-dimensional electron gas in the lower channel layer 3 is depleted through the p-type GaN gate layer 6, and finally an enhanced GaN HEMT device is obtained.

[0061] Example 2

[0062] A method for preparing an enhanced GaN HEMT device comprises the following steps:

[0063] Step 1: using a metal organic chemical vapor deposition (MOCVD) process to sequentially grow a buffer layer 2, a channel layer 3, a barrier layer 4 and a p-GaN cap layer 5 on the surface of a substrate layer 1 to obtain an epitaxial structure;

[0064] First, a 1000nm thick AlN buffer layer 2 is grown on the substrate layer 1 at a low temperature of 500°C; at a temperature of 1000°C, a 600nm thick AlGaN channel layer 3 is grown on the AlN buffer layer 2, and a 10nm thick AlGaN barrier layer 4 is epitaxially grown on the AlGaN channel layer 3, with an Al component of 0.15 and a Ga component of 0.85; finally, a p-GaN cap layer 5 is epitaxially grown on the AlGaN barrier layer 4, with Mg doping and a doping concentration of 5×10 17 cm -3 , with a thickness of 50nm; the material of the substrate layer 1 is SiC, with a thickness of 500μm;

[0065] Step 2: Soak the epitaxial structure obtained in step 1 in a mixed solution of H2SO4 and H2O2 with a volume ratio of 7:3 for 1 minute to remove oxides and impurities on the surface of the epitaxial structure, and then perform organic cleaning in acetone solution and isopropanol solution for 5 minutes by ultrasonic treatment.

[0066] Step 3: Photolithography is performed on the surface of the epitaxial structure cleaned in step 2 by using a photoresist reversal process to obtain a photoresist pattern in the gate region; then a layer of Au is further deposited on the surface of the epitaxial structure by an electron beam evaporation process, and a mask layer outside the gate region is obtained after peeling off;

[0067] Step 4: using an electron beam device to irradiate the gate region on the surface of the epitaxial structure not covered by the mask layer in step 3 with an electron beam to activate the Mg impurities therein, and then cleaning the mask layer to obtain a p-type GaN gate 6; the acceleration voltage of the electron beam is 35 kV, the emission current is 20 μA, and the beam size is 75 μm;

[0068] Step 5: Use a photoresist process to perform photolithography on the surface of the structure obtained in step 4 to obtain a photoresist pattern in the mesa area; use a semiconductor material etcher ICP to perform etching with an etching depth of 200nm to form a mesa isolation, such as Figure 4 As shown;

[0069] Step 6: Photolithography is performed on the surface of the structure obtained in step 5 by using a photoresist reversal process to obtain a photoresist pattern outside the source and drain electrode regions; then, a semiconductor material etcher (ICP) is used for etching to remove the p-GaN in the source and drain electrode regions; then, Ti, Al, Ni, and Au are grown in sequence by an electron beam evaporation process, wherein the thickness of Ti is 20 nm, the thickness of Al is 120 nm, the thickness of Ni is 45 nm, and the thickness of Au is 55 nm, and source electrode 7 and drain electrode 8 are formed after peeling;

[0070] Step 7: The device obtained in step 6 is subjected to rapid thermal annealing in a N2 atmosphere at 800°C for 35 seconds, so that the source electrode 7 and the drain electrode 8 form an ohmic contact with the barrier layer 4;

[0071] Step 8: Photolithography is performed on the surface of the structure obtained in step 7 by using a photoresist reversal process to obtain a photoresist pattern outside the gate metal electrode area; then Ni and Au are grown in sequence by an electron beam evaporation process, wherein the thickness of Ni is 30 nm and the thickness of Au is 120 nm, and a gate metal electrode 9 is obtained after peeling; the gate metal electrode 9 forms a Schottky contact with the p-type GaN gate 6, and the two-dimensional electron gas in the lower channel layer 3 is depleted through the p-type GaN gate layer 6, and finally an enhanced GaN HEMT device is obtained.

[0072] Example 3

[0073] A method for preparing an enhanced GaN HEMT device comprises the following steps:

[0074] Step 1: using a metal organic chemical vapor deposition (MOCVD) process to sequentially grow a buffer layer 2, a channel layer 3, a barrier layer 4 and a p-GaN cap layer 5 on the surface of a substrate layer 1 to obtain an epitaxial structure;

[0075] First, a 5000nm thick AlGaN buffer layer 2 is grown on the substrate layer 1 at a low temperature of 500°C; at a temperature of 1000°C, a 900nm thick InGaN channel layer 3 is grown on the AlGaN buffer layer 2, and a 25nm thick AlGaN barrier layer 4 is epitaxially grown on the InGaN channel layer 3, with an Al component of 0.05 and a Ga component of 0.95; finally, a p-GaN cap layer 5 is epitaxially grown on the AlGaN barrier layer 4, with Mg doping and a doping concentration of 5×10 20 cm -3 , with a thickness of 130nm; the material of the substrate layer 1 is sapphire, with a thickness of 1000μm;

[0076] Step 2: Soak the epitaxial structure obtained in step 1 in a mixed solution of H2SO4 and H2O2 with a volume ratio of 7:3 for 1 minute to remove oxides and impurities on the surface of the epitaxial structure, and then perform organic cleaning in acetone solution and isopropanol solution for 5 minutes by ultrasonic treatment.

[0077] Step 3: Photolithography is performed on the surface of the epitaxial structure cleaned in step 2 by using a photoresist reversal process to obtain a photoresist pattern in the gate region; then a layer of Au is further deposited on the surface of the epitaxial structure by an electron beam evaporation process, and a mask layer outside the gate region is obtained after peeling off;

[0078] Step 4: using an electron beam device to irradiate the gate region on the surface of the epitaxial structure not covered by the mask layer in step 3 with an electron beam to activate the Mg impurities therein, and then cleaning the mask layer to obtain a p-type GaN gate 6; the acceleration voltage of the electron beam is 40 kV, the emission current is 80 μA, and the beam size is 140 μm;

[0079] Step 5: Use a photoresist process to perform photolithography on the surface of the structure obtained in step 4 to obtain a photoresist pattern in the mesa area; use a semiconductor material etcher ICP to perform etching with an etching depth of 200nm to form a mesa isolation, such as Figure 4 As shown;

[0080] Step 6: Photolithography is performed on the surface of the structure obtained in step 5 by using a photoresist reversal process to obtain a photoresist pattern outside the source and drain electrode regions; then, a semiconductor material etcher (ICP) is used for etching to remove the p-GaN in the source and drain electrode regions; then, Ti, Al, Ni, and Au are grown in sequence by an electron beam evaporation process, wherein the thickness of Ti is 20 nm, the thickness of Al is 120 nm, the thickness of Ni is 45 nm, and the thickness of Au is 55 nm, and source electrode 7 and drain electrode 8 are formed after peeling;

[0081] Step 7: The device obtained in step 6 is rapidly thermally annealed in a N2 atmosphere at 850°C for 30s to form an ohmic contact between the source electrode 7 and the drain electrode 8 and the barrier layer 4;

[0082] Step 8: Photolithography is performed on the surface of the structure obtained in step 7 by using a photoresist reversal process to obtain a photoresist pattern outside the gate metal electrode area; then Ni and Au are grown in sequence by an electron beam evaporation process, wherein the thickness of Ni is 30 nm and the thickness of Au is 120 nm, and a gate metal electrode 9 is obtained after peeling; the gate metal electrode 9 forms a Schottky contact with the p-type GaN gate 6, and the two-dimensional electron gas in the lower channel layer 3 is depleted through the p-type GaN gate layer 6, and finally an enhanced GaN HEMT device is obtained.

Claims

1. A method for preparing an enhanced GaN HEMT device, Features: The steps include: Step 1: using a metal organic chemical vapor deposition (MOCVD) process to sequentially grow a buffer layer (2), a channel layer (3), a barrier layer (4) and a p-GaN cap layer (5) on the surface of a substrate layer (1) to obtain an epitaxial structure; Step 2: Photolithography is performed on the surface of the epitaxial structure in step 1 by using a photoresist reversal process to obtain a photoresist pattern in the gate region; then a layer of Au is further deposited on the surface of the epitaxial structure by an electron beam evaporation process, and a mask layer outside the gate region is obtained after peeling off; Step 3: using an electron beam device to perform electron beam irradiation on the gate region of the epitaxial structure surface in step 2 that is not covered by the mask layer to activate the Mg impurities therein, and then cleaning the mask layer to obtain a p-type GaN gate (6); Step 4: Photolithography is performed on the surface of the structure obtained in step 3 using a photoresist process to obtain a photoresist pattern in the mesa area; Then, a semiconductor material etcher (ICP) is used for etching, and the etching depth starts from the p-GaN cap layer (5) until a portion of the channel layer (3) is etched away to form a mesa isolation; Step 5: performing photolithography on the surface of the structure obtained in step 4 using a photoresist reversal process to obtain a photoresist pattern outside the source and drain electrode region; Then, a semiconductor material etcher (ICP) is used for etching to remove the p-GaN and AlGaN in the source and drain electrode regions; then, an electron beam evaporation process is used for metal evaporation, and after stripping, a source electrode (7) and a drain electrode (8) are obtained; Step 6: For the device obtained in step 5, 2 Performing rapid thermal annealing in an atmosphere to form an ohmic contact between the source electrode (7) and the drain electrode (8) and the barrier layer (4); Step 7: photolithography is performed on the surface of the structure obtained in step 6 by using a photoresist reversal process to obtain a photoresist pattern other than the gate metal electrode; then metal evaporation is performed by using an electron beam evaporation process, and a gate metal electrode (9) is obtained after stripping; the gate metal electrode (9) forms a Schottky contact with the p-type GaN gate (6), and the two-dimensional electron gas in the lower channel layer (3) is depleted through the p-type GaN gate (6), and finally an enhanced GaN HEMT device is obtained.

2. The method for preparing an enhanced-mode GaN HEMT device according to claim 1, Features: In step 1, the material of the substrate layer (1) is Si, SiC, sapphire or diamond, with a thickness of 100-1500 μm; the material of the buffer layer (2) is AlN, GaN or AlGaN, with a thickness of 1000-6000 nm; the material of the channel layer (3) is GaN, AlGaN or InGaN, with a thickness of 200-1000 nm; the material of the barrier layer (4) is AlGaN, with a thickness of 10-25 nm, and an Al component of 0.05-0.25; the material of the p-GaN cap layer (5) is GaN, with a thickness of 50-140 nm, and the doping impurity is Mg, and the doping concentration is 5×10 17 – 5x10 20 cm -3 .

3. The method for preparing an enhanced-mode GaN HEMT device according to claim 1, Features: The epitaxial structure obtained in step 1 was placed in a H 2 SO 4 and H 2 O 2 The surface of the epitaxial structure is then immersed in a mixed solution to remove oxides and impurities, and then organic cleaning is performed in acetone solution and isopropanol solution in sequence.

4. The method for preparing an enhanced-mode GaN HEMT device according to claim 1, Features: In step 4, the acceleration voltage of the electron beam is 10-50 kV, the emission current is 20-100 μA, and the beam size is 5-150 μm.

5. The method for preparing an enhancement mode GaN HEMT device according to claim 1, It is characterized in that In the step 5, the structures of the source electrode (7) and the drain electrode (8) are Ti / Al / Ni / Au from bottom to top, and the thicknesses are 20 / 120 / 45 / 55 nm, respectively.

6. The method for preparing an enhancement mode GaN HEMT device according to claim 1, Features: In step 6, the annealing temperature is 800-850° C., and the annealing time is 30-35 seconds.

7. The method for preparing an enhancement mode GaN HEMT device according to claim 1, It is characterized in that The structures of the gate metal electrode (9) in step 7 are Ni / Au from bottom to top, and the thicknesses are 30 / 120 nm.

8. The method for preparing an enhancement mode GaN HEMT device according to claim 1, It is characterized in that After the photolithography operation in step 7, magnetron sputtering technology can be used to deposit W or TiN to obtain a gate metal electrode (9).

9. An enhancement mode GaN HEMT device, Features: The method is described in any one of claims 1 to 8.

Citation Information

Patent Citations

  • Compound semiconductor device and method for manufacturing the same

    CN103000666A

  • High-resistance cap layer-based III-nitride polarization super-junction high electron mobility transistor (HEMT) device and fabrication method thereof

    CN106981513A

  • Enhanced power device and manufacturing method thereof

    CN111477547A