Double-sided polycrystalline battery

By setting a polycrystalline layer on both sides of the battery and performing passivation and anti-reflection layer processing, the problem of high recombination of the front gate line contact area is solved, which significantly improves the efficiency and performance of the battery.

CN119050176APending Publication Date: 2024-11-29江苏中清先进电池制造有限公司
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411516346.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-29
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

In the prior art, the recombination of the front gate line contact area is relatively high, which affects the battery efficiency, and there are significant differences in the recombination of the back passivation contact area.

Method used

A double-sided polycrystalline cell structure is adopted, in which a polycrystalline layer is provided on the front and back of the N-type silicon wafer, and the embedded connection with the anti-reflection layer is reduced by passivation, and the contact area is recombined, and chemical treatment and laser treatment are adopted. A polycrystalline layer is formed and an electrode is formed in combination with metallization.

Benefits of technology

It significantly improves the open circuit voltage and filling factor of the battery, improves the battery efficiency, reduces the recombination of the contact area, and improves the overall performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050176A_ABST
    Figure CN119050176A_ABST
Patent Text Reader

Abstract

A double-sided polycrystalline battery belongs to the technical field of batteries and comprises an N-type silicon wafer and polycrystalline layers arranged on two sides of the N-type silicon wafer, and the polycrystalline layers comprise a front polycrystalline layer and a back polycrystalline layer. The front surface of the N-type silicon wafer comprises a graphic area and a non-graphic area, a front polycrystal layer is arranged on the graphic area, and passivation and antireflection layers are respectively arranged on the front polycrystal layer and the non-graphic area; a back polycrystal layer is arranged on the back of the N-type silicon wafer, and a passivation and antireflection layer is arranged on the back polycrystal layer; wherein the front polycrystal layer and the back polycrystal layer are configured as follows: when the front polycrystal layer is a p-polycrystal layer, the back polycrystal layer is an n-polycrystal layer, and when the front polycrystal layer is an n-polycrystal layer, the back polycrystal layer is a p-polycrystal layer; the open-circuit voltage and the filling factor of the battery are remarkably improved, and the working efficiency of the battery is remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of batteries, and specifically refers to a double-sided polycrystalline battery and a manufacturing method thereof. Background Art

[0002] The existing topcon (Tunnel Oxide Passivating Contact) cell technology uses a tunnel oxide layer superimposed with a doped polycrystalline (polycrystalline) structure to form a passivation contact on the back, which greatly reduces the recombination of the back surface and improves the cell efficiency; however, the front grid line contact area is still in direct contact with the silver paste and silicon, and the recombination is relatively high; although the industry currently uses LECO (Laser-enhanced contact optimization, laser assisted sintering) technology to reduce recombination, the recombination in the contact area still reaches 200fA / mm2, which is significantly higher than the passivation contact area of ​​less than 50fA / mm2. Therefore, how to reduce the recombination in the front contact area in the front grid line contact area to improve the cell efficiency is a hot topic in research and development. Summary of the invention

[0003] In view of the above situation, in order to overcome the defects of the prior art, the embodiments of the present invention provide a double-sided multi-crystalline battery and a manufacturing method thereof, which at least partially solve the above technical problems.

[0004] The technical solution adopted by the embodiment of the present invention is as follows: a bifacial polycrystalline cell, comprising an N-type silicon wafer, and polycrystalline layers arranged on both sides of the N-type silicon wafer, wherein the polycrystalline layers include a front polycrystalline layer and a back polycrystalline layer; The front side of the N-type silicon wafer includes a graphic area and a non-graphic area, the graphic area is provided with a front polycrystalline layer, and the front polycrystalline layer and the non-graphic area are respectively provided with a passivation layer and an anti-reflection layer; A back polycrystalline layer is provided on the back side of the N-type silicon wafer, and a passivation and anti-reflection layer is provided on the back polycrystalline layer; Wherein, the front polycrystalline layer and the back polycrystalline layer are configured as follows: When the front polycrystalline layer is a p-polycrystalline layer, the back polycrystalline layer is an n-polycrystalline layer, and when the front polycrystalline layer is an n-polycrystalline layer, the back polycrystalline layer is a p-polycrystalline layer.

[0005] Preferably, when the front polycrystalline layer is a p-polycrystalline layer and the back polycrystalline layer is an n-polycrystalline layer, the preparation method comprises the following steps: Double-sided polishing after chemical treatment on N-type silicon wafers; Amorphous silicon is deposited on the front side of the N-type silicon wafer to form a front i-polycrystalline layer, and the non-patterned area is subjected to texturing treatment; Diffusion of boron is performed on the front i-polycrystalline layer to form a p-polycrystalline layer, wherein a PN junction is formed between the p-polycrystalline layer and the N-type silicon wafer; Amorphous silicon is deposited on the back of the N-type silicon wafer to form a back i-polycrystalline layer, and then phosphorus is doped to form an n-polycrystalline layer; Remove impurities from the front and edge of the N-type silicon wafer through wet cleaning; After metallization treatment, the front electrode and the back electrode are formed to form a double-sided polycrystalline battery structure.

[0006] Further, after amorphous silicon is deposited on the front side of the N-type silicon wafer to form a front side i-polycrystalline layer, a mask is deposited on the i-polycrystalline layer; The mask on the non-patterned area is ablated by laser treatment, and after ablation, a texturing treatment is performed on the non-patterned area.

[0007] Furthermore, the texturing process is specifically as follows: The non-graphic area is subjected to texturing treatment by using alkali and texturing additives, wherein the alkali is sodium hydroxide.

[0008] Further, before depositing amorphous silicon on the back side of the N-type silicon wafer; The BSG layer on the back of the N-type silicon wafer is firstly removed by pickling with hydrofluoric acid and then alkaline polishing with sodium hydroxide.

[0009] Preferably, when the front polycrystalline layer is an n-polycrystalline layer and the back polycrystalline layer is a p-polycrystalline layer, the preparation method includes the following steps: Double-sided polishing after chemical treatment on N-type silicon wafers; Depositing amorphous silicon on the back side of the N-type silicon wafer to form a back side i-polycrystalline layer; Boron diffusion is performed on the back i-poly layer to form a p-poly layer; Amorphous silicon is deposited on the front side of the N-type silicon wafer to form a front i-polycrystalline layer, phosphorus is diffused on the i-polycrystalline layer to form an n-polycrystalline layer, and a non-patterned area is cleaned and textured; After metallization treatment, the front electrode and the back electrode are formed to form a double-sided polycrystalline battery structure.

[0010] Preferably, before amorphous silicon is deposited on the front side of the N-type silicon wafer, the front side of the N-type silicon wafer is polished; The BSG and P++ layers on the front side of the N-type silicon wafer are firstly removed by pickling with hydrofluoric acid and then alkaline polishing with sodium hydroxide.

[0011] Preferably, a mask is deposited on the front side of the N-type silicon wafer, the mask on the non-patterned area is ablated by laser treatment, and after ablation, the non-patterned area is subjected to texturing treatment by alkali and texturing additives.

[0012] Preferably, before the metallization treatment, the N-type silicon wafer needs to be subjected to double-sided aluminum oxide ALD passivation treatment and double-sided coating treatment.

[0013] Preferably, it also includes a front electrode and a back electrode, the front electrode passes through the passivation and anti-reflection layer on the front polycrystalline layer and is embedded in the front polycrystalline layer, and the back electrode passes through the passivation and anti-reflection layer on the back polycrystalline layer and is embedded in the back polycrystalline layer.

[0014] Preferably, the passivation and anti-reflection layer comprises an aluminum oxide layer and a coating layer, and the coating layer is arranged on the aluminum oxide layer; The coating layer includes one or more combinations of silicon nitride, silicon oxynitride, and silicon oxide.

[0015] The beneficial effects achieved by the present invention using the above structure are as follows: The present invention uses a passivated contact structure in both the front grid line contact area and the back area, which reduces the recombination of the contact areas on both sides of the battery, significantly improves the open circuit voltage and fill factor of the battery, and thus greatly improves the efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 A schematic diagram of the structure of a double-sided multicrystalline battery prepared in an embodiment of the present invention; In the figure: the front poly layer is the front polycrystalline layer, and the back poly layer is the back polycrystalline layer.

[0017] The accompanying drawings are used to provide further understanding of the embodiments of the present invention and constitute a part of the specification. They are used to explain the present invention together with the embodiments of the present invention and do not constitute a limitation of the present invention. DETAILED DESCRIPTION

[0018] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments; based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0019] In the description of the embodiments of the present invention, it should be understood that terms such as "up", "down", "front", "back", "left", "right", "top", "bottom", "inside" and "outside" indicating directions or positional relationships are based on the directions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the embodiments of the present invention and simplifying the description, rather than indicating or implying that the referred device or element must have a specific direction, be constructed and operated in a specific direction, and therefore should not be understood as limiting the present invention.

[0020] like Figure 1As shown, a bifacial polycrystalline cell comprises an N-type silicon wafer and polycrystalline layers arranged on both sides of the N-type silicon wafer, wherein the polycrystalline layers comprise a front polycrystalline layer and a back polycrystalline layer; The front side of the N-type silicon wafer includes a graphic area and a non-graphic area, the graphic area is provided with a front polycrystalline layer, and the front polycrystalline layer and the non-graphic area are respectively provided with a passivation layer and an anti-reflection layer; A back polycrystalline layer is provided on the back side of the N-type silicon wafer, and a passivation and anti-reflection layer is provided on the back polycrystalline layer.

[0021] It also includes a front electrode and a back electrode. The front electrode passes through the passivation and anti-reflection layer on the front polycrystalline layer and is embedded in the front polycrystalline layer. The back electrode passes through the passivation and anti-reflection layer on the back polycrystalline layer and is embedded in the back polycrystalline layer.

[0022] It should be noted that the front electrode and the back electrode of the battery are respectively embedded in the polycrystalline layer provided on the N-type silicon wafer through the passivation and anti-reflection layer provided on the N-type silicon wafer of the battery. In the process of electrochemical preparation of porous silicon, an electrochemical corrosion method is required, and at this time, the electrode needs to pass through the anti-reflection layer.

[0023] In addition, the electrode passing through the anti-reflection layer will also affect the microstructure and optical properties of porous silicon, as well as determine the time interval for the formation of porous silicon and characterize the micromorphology of porous silicon. By testing the anti-reflection performance of the porous silicon layer, the electrochemical corrosion parameters suitable for anti-reflection of solar cells can be determined.

[0024] In a further implementation of this embodiment, the passivation and anti-reflection layer includes an aluminum oxide layer and a coating layer, and the coating layer is disposed on the aluminum oxide layer; The coating layer includes one or more combinations of silicon nitride, silicon oxynitride, and silicon oxide.

[0025] It should be noted that the passivation and anti-reflection layers can protect the battery from corrosion and improve the photoelectric conversion efficiency; The passivation layer can prevent the metal surface from corrosion. In an electrochemical environment, the passivation layer changes the electrode potential of the metal surface, making the metal lose the ability to participate in the corrosion reaction.

[0026] The anti-reflection layer can reduce the reflection of incident light and improve the photoelectric conversion efficiency. By reducing the surface reflectivity, more light energy can be absorbed, thereby improving the energy conversion efficiency of the battery.

[0027] It should be noted that the polycrystalline layer includes an n-polycrystalline layer and a p-polycrystalline layer. The front polycrystalline layer and the back polycrystalline layer of an N-type silicon wafer are configured as follows: when the front polycrystalline layer of an N-type silicon wafer is an n-polycrystalline layer, the back polycrystalline layer is a p-polycrystalline layer.

[0028] It should be noted that: in this solution, both sides of the battery can be polycrystalline treated separately, and the polycrystalline layers on both sides can be selected, which increases the applicability range of battery preparation.

[0029] When the front polycrystalline layer of an N-type silicon wafer is a p-polycrystalline layer, the back polycrystalline layer is an n-polycrystalline layer; By processing the battery on both sides with polycrystalline, the open circuit voltage and fill factor of the battery can be greatly improved, thereby greatly improving the efficiency of the battery.

[0030] In a further implementation of this embodiment, when the front polycrystalline layer is a p-polycrystalline layer and the back polycrystalline layer is an n-polycrystalline layer, the preparation method thereof comprises the following steps: Double-sided polishing after chemical treatment on N-type silicon wafers; Amorphous silicon is deposited on the front side of the N-type silicon wafer to form a front i-polycrystalline layer, and the non-patterned area is subjected to texturing treatment; Diffusion of boron is performed on the front i-polycrystalline layer to form a p-polycrystalline layer, wherein a PN junction is formed between the p-polycrystalline layer and the N-type silicon wafer; Amorphous silicon is deposited on the back of the N-type silicon wafer to form a back i-polycrystalline layer, and then phosphorus is doped to form an n-polycrystalline layer; Remove impurities from the front and edge of the N-type silicon wafer through wet cleaning; After metallization treatment, the front electrode and the back electrode are formed to form a double-sided polycrystalline battery structure.

[0031] In a further implementation of this embodiment, after amorphous silicon is deposited on the front side of the N-type silicon wafer to form a front side i-polycrystalline layer, a mask is deposited on the i-polycrystalline layer; The mask on the non-patterned area is ablated by laser treatment, and after ablation, a texturing treatment is performed on the non-patterned area.

[0032] In a further implementation of this embodiment, the texturing process is specifically: The non-graphic area is subjected to texturing treatment by using alkali and texturing additives, wherein the alkali is sodium hydroxide.

[0033] In a further implementation of this embodiment, before depositing amorphous silicon on the back side of the N-type silicon wafer; The BSG layer on the back of the N-type silicon wafer is firstly removed by pickling with hydrofluoric acid and then alkaline polishing with sodium hydroxide.

[0034] It should be noted that: wet chemical treatment is performed on N-type silicon wafers to perform double-sided polishing; Then, the front amorphous silicon is formed into an i-polycrystalline layer, and then a mask is deposited on the i-polycrystalline layer; Then, the non-graphic area mask is ablated with a laser, followed by a texturing process to form a pyramid-shaped velvet surface, wherein the texturing process is performed by adding alkali (sodium hydroxide) and texturing additives.

[0035] Then boron diffusion square resistor is carried out to form the front PN junction, the back BSG layer is removed by acid (hydrofluoric acid) washing and then alkaline polishing, and then amorphous silicon is deposited on the back to form an i-polycrystalline layer.

[0036] Then phosphorus doping is performed on the back to form an N+ layer, and RCA is performed to remove the N+ layer on the front and edges. Then double-sided aluminum oxide ALD and double-sided coating (silicon nitride, silicon oxynitride, silicon oxide) are processed for passivation and anti-reflection, and finally metallization treatment is performed to form electrodes, ultimately forming the front battery structure.

[0037] The double-sided multicrystalline cell manufactured in this embodiment has the same back side as the existing cell, and the back side is polished, and then a tunneling oxide layer is made, and N-type doped polysilicon is made on the tunneling layer. A patterned tunneling oxide layer and an i-polycrystalline layer are first formed on the front side in an area corresponding to the gate line pattern, and a velvet structure is formed on the surface of the silicon wafer in the remaining area.

[0038] The silicon wafer is then sent to a boron diffusion machine for boron diffusion, so that the velvet area and the i-polycrystalline area are diffused at the same time.

[0039] Among them, the square resistance of the velvet area is 200~500Ω, and the square resistance of the polycrystalline area is 30~400Ω. Then the front and back sides are coated, and the gate lines are printed on the front and back sides to form a finished battery cell. Through one-time boron diffusion, the square resistance of the velvet area is 200~500Ω, and the square resistance of the polycrystalline area is 30~400Ω. A positive junction is formed on the front side, and a P-polycrystalline passivation contact structure is formed in the polycrystalline area. The open circuit voltage and fill factor efficiency of the battery can be significantly improved by 0.4%.

[0040] In a further implementation of this embodiment, when the front polycrystalline layer is an n-polycrystalline layer and the back polycrystalline layer is a p-polycrystalline layer, the preparation method thereof comprises the following steps: Double-sided polishing after chemical treatment on N-type silicon wafers; Depositing amorphous silicon on the back side of the N-type silicon wafer to form a back side i-polycrystalline layer; Boron diffusion is performed on the back i-poly layer to form a p-poly layer; Amorphous silicon is deposited on the front side of the N-type silicon wafer to form a front i-polycrystalline layer, phosphorus is diffused on the i-polycrystalline layer to form an n-polycrystalline layer, and a non-patterned area is cleaned and textured; After metallization treatment, the front electrode and the back electrode are formed to form a double-sided polycrystalline battery structure.

[0041] In a further implementation of this embodiment, before amorphous silicon is deposited on the front side of the N-type silicon wafer, the front side of the N-type silicon wafer is polished; The BSG and P++ layers on the front side of the N-type silicon wafer are firstly removed by pickling with hydrofluoric acid and then alkaline polishing with sodium hydroxide.

[0042] In a further implementation of this embodiment, a mask is deposited on the front side of the N-type silicon wafer, the mask on the non-patterned area is ablated by laser treatment, and after ablation, the non-patterned area is textured by alkali and a texturing additive.

[0043] In a further implementation of this embodiment, the N-type silicon wafer needs to be subjected to double-sided aluminum oxide ALD passivation treatment and double-sided coating treatment before the metallization treatment.

[0044] It should be noted that wet chemical treatment is performed on N-type silicon wafers and double-sided polishing is performed.

[0045] Then, amorphous silicon is formed on the back side to form an i-polycrystalline layer, followed by boron diffusion to form a P-polycrystalline layer, and then the front side is polished to remove the front BSG and P++ layers.

[0046] Then, amorphous silicon is deposited on the front side to form an i-polycrystalline layer, followed by P diffusion to form an n-polycrystalline layer.

[0047] Then the front side is patterned, cleaned and textured, the front PSG layer is removed and a pyramid texture surface is generated, followed by double-sided ALD passivation and double-sided coating, passivation and anti-reflection, and finally metallization treatment to form electrodes, ultimately forming the battery structure on the back side.

[0048] The bifacial polycrystalline cell manufactured in this embodiment is different from the above-mentioned cell embodiment with a front PN junction in that an n-polycrystalline layer is formed on the front side and a p-polycrystalline layer is formed on the back side; It can also significantly improve the open circuit voltage and fill factor of the battery, and the efficiency can be increased by 0.4%. Example

[0049] The embodiment of the present invention proposes a double-sided multicrystalline battery, which selects an N-type silicon wafer with a resistivity of 0.4-3Ω / cm and performs double-sided polishing. The silicon wafer is placed in an LPCVD and oxygen is first passed through it before polishing to form a 1nm silicon oxide layer. The vacuum is then drawn and a mixed gas of silane and phosphine is passed through it to form a 15nm doped amorphous silicon layer. The vacuum is drawn and silane is passed through it to form a 130nm amorphous silicon layer.

[0050] Then comes mask deposition, laser and texturing.

[0051] The silicon wafer was placed in a diffusion furnace and heated to 870°C. 3000 sccm of BCL3 with 300 sccm was introduced for 15 minutes. Then the source was stopped and the temperature was maintained for 40 minutes for diffusion advancement.

[0052] The back side is alkaline polished, amorphous silicon is deposited (consistent with the first step of polycrystalline), phosphorus diffusion is performed, and RCA cleaning is performed.

[0053] Al2O3 and SixNy are deposited on both sides, and the grid electrodes are printed and sintered to finally form a battery cell. Example

[0054] The present invention proposes a double-sided multicrystalline battery, wherein an N-type silicon wafer with a resistivity of 0.4-3Ω / cm is selected and double-sided polishing is performed. The silicon wafer is placed in an LPCVD and oxygen is first passed through it before polishing to form a 1nm silicon oxide layer. The silicon wafer is then vacuumed and a mixed gas of silane and phosphine is passed through it to form a 15nm doped amorphous silicon layer. The silicon wafer is then vacuumed and silane is passed through it to form a 130nm amorphous silicon layer.

[0055] The silicon wafer was placed in a diffusion furnace and heated to 870°C. 3000 sccm of BCL3 with 300 sccm was introduced for 15 minutes. Then the source was stopped and the temperature was maintained for 40 minutes for diffusion advancement.

[0056] The back side is alkaline polished, amorphous silicon is deposited on the front side (consistent with the first step of polycrystalline), the silicon wafer is placed in a high-temperature furnace for phosphorus doping process, and the front side is patterned and textured.

[0057] Al2O3 and SixNy are deposited on both sides, and the grid electrodes are printed and sintered to finally form a battery cell.

[0058] It should be noted that, in this article, the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.

[0059] The present invention and its embodiments are described above, and such description is not restrictive. The drawings show only one embodiment of the present invention, and the actual structure is not limited thereto. In short, if ordinary technicians in the field are inspired by it, without departing from the creative purpose of the embodiments of the present invention, they can design a structure and embodiment similar to the technical solution without creativity, which should belong to the protection scope of the present invention.

Claims

1. A bifacial multicrystalline cell, characterized in that: Including N-type silicon wafer; The front side of the N-type silicon wafer includes a graphic area and a non-graphic area, the graphic area is provided with a front polycrystalline layer, and the front polycrystalline layer and the non-graphic area are both provided with a passivation and anti-reflection layer; A back polycrystalline layer is provided on the back side of the N-type silicon wafer, and a passivation and anti-reflection layer is provided on the back polycrystalline layer; Wherein, the front polycrystalline layer and the back polycrystalline layer are configured as follows: When the front polycrystalline layer is a p-polycrystalline layer, the back polycrystalline layer is an n-polycrystalline layer, and when the front polycrystalline layer is an n-polycrystalline layer, the back polycrystalline layer is a p-polycrystalline layer.

2. The bifacial multicrystalline cell according to claim 1, characterized in that: When the front polycrystalline layer is a p-polycrystalline layer and the back polycrystalline layer is an n-polycrystalline layer, the preparation method comprises the following steps: Double-sided polishing after chemical treatment on N-type silicon wafers; Amorphous silicon is deposited on the front side of the N-type silicon wafer to form a front i-polycrystalline layer, and the non-patterned area is subjected to texturing treatment; Diffusion of boron is performed on the front i-polycrystalline layer to form a p-polycrystalline layer, wherein a PN junction is formed between the p-polycrystalline layer and the N-type silicon wafer; Amorphous silicon is deposited on the back of the N-type silicon wafer to form a back i-polycrystalline layer, and then phosphorus is doped to form an n-polycrystalline layer; Remove impurities from the front and edge of the N-type silicon wafer through wet cleaning; After metallization treatment, the front electrode and the back electrode are formed to form a double-sided polycrystalline battery structure.

3. The bifacial multicrystalline cell according to claim 2, characterized in that: After amorphous silicon is deposited on the front side of the N-type silicon wafer to form a front i-polycrystalline layer, a mask is deposited on the i-polycrystalline layer; The mask on the non-patterned area is ablated by laser treatment, and after ablation, a texturing treatment is performed on the non-patterned area.

4. The bifacial multicrystalline cell according to claim 2, characterized in that: The texturing process is specifically as follows: The non-graphic area is subjected to texturing treatment by using alkali and a texturing additive, wherein the alkali is sodium hydroxide; Before amorphous silicon deposition on the back side of an N-type silicon wafer; The BSG layer on the back of the N-type silicon wafer is firstly removed by pickling with hydrofluoric acid and then alkaline polishing with sodium hydroxide.

5. The double-sided multicrystalline cell according to claim 1, characterized in that: When the front polycrystalline layer is an n-polycrystalline layer and the back polycrystalline layer is a p-polycrystalline layer, the preparation method includes the following steps: Double-sided polishing after chemical treatment on N-type silicon wafers; Depositing amorphous silicon on the back side of the N-type silicon wafer to form a back side i-polycrystalline layer; Boron diffusion is performed on the back i-poly layer to form a p-poly layer; Amorphous silicon is deposited on the front side of the N-type silicon wafer to form a front i-polycrystalline layer, phosphorus is diffused on the i-polycrystalline layer to form an n-polycrystalline layer, and a non-patterned area is cleaned and textured; After metallization treatment, the front electrode and the back electrode are formed to form a double-sided polycrystalline battery structure.

6. The double-sided multicrystalline cell according to claim 5, characterized in that: Before amorphous silicon is deposited on the front side of the N-type silicon wafer, the front side of the N-type silicon wafer is polished; First, pickle with hydrofluoric acid and then use sodium hydroxide to alkaline polish to remove the BSG and P++ layers on the front side of the N-type silicon wafer; A mask is deposited on the front side of an N-type silicon wafer, and the mask on the non-patterned area is ablated by laser treatment. After ablation, the non-patterned area is textured by alkali and a texturing additive.

7. The bifacial multicrystalline cell according to claim 2 or 5, characterized in that: Before metallization, the N-type silicon wafer needs to be subjected to double-sided aluminum oxide ALD passivation treatment and double-sided coating treatment.

8. The double-sided multicrystalline cell according to claim 7, characterized in that: It also includes a front electrode and a back electrode. The front electrode passes through the passivation and anti-reflection layer on the front polycrystalline layer and is embedded in the front polycrystalline layer. The back electrode passes through the passivation and anti-reflection layer on the back polycrystalline layer and is embedded in the back polycrystalline layer.

9. The double-sided multicrystalline cell according to claim 1, characterized in that: The passivation and anti-reflection layer comprises an aluminum oxide layer and a coating layer, and the coating layer is arranged on the aluminum oxide layer; The coating layer includes one or more combinations of silicon nitride, silicon oxynitride, and silicon oxide.

Citation Information

Patent Citations

  • Double-sided doped polycrystalline silicon passivation contact battery and preparation method thereof

    CN116914012A

  • Front surface local polycrystalline silicon passivation contact crystalline silicon solar cell and preparation method thereof

    CN118486757A

  • Efficient TOPCon battery and preparation method thereof

    CN118553800A