Composite lithium metal negative electrode, preparation method thereof and solid-state battery
By generating Li-Al alloy and Li3N in lithium metal batteries, a high ion conductive network is constructed, the interface cavity problem of lithium metal batteries is solved, the lithium diffusion rate and interface stability are improved, and a solid-state lithium metal battery with high energy density is realized.
Patent Information
- Application Number
- CN202411236751.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-29
AI Technical Summary
Solid-state lithium metal batteries have poor rate performance and limitations of lithium dendrites due to the formation of cavity at the interface between lithium metal and solid electrolyte. The prior art is difficult to effectively suppress the growth of lithium cavities, resulting in interface instability and low lithium utilization.
By reacting trace amounts of aluminum nitrate with molten lithium metal to form Li-Al alloy and Li3N, an ion transmission network with high ion conductivity is constructed, the lithium diffusion rate and interface contact ability are improved, and the composite lithium metal negative electrode is prepared to inhibit the formation of lithium cavity.
The close contact between lithium metal and garnet solid electrolyte is achieved, the formation of lithium cavity is avoided, the lithium diffusion rate and interface stability is improved, the battery cycle life is extended, and the energy density is improved.
Smart Images

Figure CN119050284A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of solid-state lithium metal batteries, and specifically relates to a composite lithium metal negative electrode and a preparation method thereof, and a solid-state battery. Background Art
[0002] Solid-state batteries have attracted great attention due to their high safety and high energy density. Lithium metal has a high specific capacity (3860 mAh g −1 ) and low electrochemical potential (−3.04 V relative to standard hydrogen electrode), it is considered to be a promising negative electrode candidate material in solid-state batteries. However, the poor rate performance of solid-state lithium metal batteries and the formation of lithium dendrites limit the practical application of lithium metal anodes. These problems are attributed to the formation of voids at the interface between lithium metal and solid electrolyte during the cycle. The lithium diffusion rate of the lithium metal bulk phase is limited. During the lithium stripping process, it is difficult for the lithium in the bulk phase to replenish the lithium consumed at the interface in time, so lithium voids are formed at the negative electrode interface. With the increase of stripping capacity, the voids gradually accumulate, resulting in the continuous deterioration of the interface contact. The accumulated lithium voids will lead to uneven electric field distribution on the interface and accelerate the uneven lithium plating on the interface, which will eventually lead to the formation of dendrites and reduce the lithium utilization rate of the negative electrode. Researchers have proposed methods such as introducing interface coatings or constructing artificial interface layers to improve the contact of the negative electrode interface and eliminate the initial lithium voids. However, this treatment is limited to the interface and does not help much for the transport of lithium in the lithium metal bulk phase. Therefore, these methods are usually only effective in the early stage of battery operation and cannot fundamentally inhibit the growth of lithium voids.
[0003] Typical prior art such as CN111224066A discloses a method for regulating the interface between a solid electrolyte and a metal lithium negative electrode, which adopts adding an appropriate amount of flux to the molten metal lithium, S3), grinding and polishing the solid electrolyte substrate; S4), placing the solid electrolyte on a heating table for heating; S5), uniformly coating the mixed molten liquid on the solid electrolyte; S6), melting the aluminum foil in the mixed molten metal liquid that is in good contact with the solid electrolyte; S7), regulating its thickness according to the amount of lithium metal required for the battery cycle; S8), cooling the product naturally to room temperature. The present invention achieves the effect of infiltration of the solid electrolyte by melting a trace amount of flux with metal lithium and coating it on the surface of the solid electrolyte, making the lithium negative electrode purer and the battery more efficient; and controlling the in-situ SEI of the surface of the solid electrolyte by adding metal aluminum foil. However, the above technology adopts the addition of metal flux to achieve electrolyte infiltration, but in the actual process, the addition of metal flux actually has many problems, such as instability.
[0004] Another typical example is the method for preparing a metallic lithium composite negative electrode disclosed in CN111509204A, which uses indium and high-viscosity alkanes to reduce the tension of lithium and achieve dispersion of lithium and other materials. However, this technology adds too much doping and it is difficult to ensure the uniformity of the battery.
[0005] Compared with the method of modifying the negative electrode interface, the use of the composite lithium metal negative electrode of the present invention is a simple and low-cost effective strategy that can effectively suppress lithium vacancies and establish close contact between the solid electrolyte and the lithium metal negative electrode. Through the reaction of molten lithium metal and aluminum nitrate, uniformly distributed Li-Al alloy, Li3N and LiNO2 are generated inside the composite lithium metal negative electrode, which construct an ion transmission network with high ionic conductivity inside the lithium metal to accelerate the migration of the negative electrode bulk lithium to the interface. At the same time, these products improve the interface contact ability between lithium metal and garnet solid electrolyte. Good interface contact and increased lithium diffusion rate can avoid the generation of lithium vacancies when lithium is stripped at the negative electrode interface, fundamentally alleviating the dynamic contact problem of unstable negative electrode interface caused by lithium vacancies growth.
[0006] This invention highlights the importance of enhancing lithium diffusion within the anode and provides a new approach for the rational design of composite lithium metal anodes to achieve high-energy-density all-solid-state batteries. Summary of the invention
[0007] The purpose of the present invention is to overcome the problem that the current lithium metal negative electrode is difficult to meet the performance requirements of energy storage equipment, and to provide a method for preparing a high-performance composite lithium metal negative electrode, a composite lithium metal negative electrode, and a solid-state lithium metal battery assembled using the method.
[0008] The purpose of the present invention can be achieved by the following technical solutions: In a first aspect, the present application provides a method for preparing a composite lithium metal negative electrode, the method comprising the following steps: 1) heating and melting metallic lithium, and removing the impurity layer on the surface of the molten lithium solution to obtain molten metallic lithium; 2) adding at least one metal salt to the molten metal lithium obtained in step 1), heating, stirring evenly, reacting fully, and cooling to room temperature to obtain a composite lithium metal negative electrode; 3) Covering the composite lithium metal negative electrode obtained in step 2) on the surface of at least one solid electrolyte and performing a heating treatment; Furthermore, the metal salt is one or more of chloride metal salts, sulfate metal salts, carbonate metal salts, and nitrate metal salts.
[0009] Furthermore, it is preferably a nitrate metal salt, and preferably the nitrate metal salt is one or more of sodium nitrate, potassium nitrate, lithium nitrate, ferric nitrate, ferrous nitrate, magnesium nitrate, aluminum nitrate, zinc nitrate, copper nitrate, bismuth nitrate, and tin nitrate.
[0010] Furthermore, in step 2), the mass of the metal salt is 1-9% of the mass of the molten lithium metal.
[0011] Furthermore, in step 1), the heating temperature of the metallic lithium is 180-260°C.
[0012] Furthermore, the stirring time in step 2) is 2-20 min, preferably 7-10 min.
[0013] Furthermore, the heating temperature in step 2) is 220°C-280°C, preferably 240°C-260°C.
[0014] Furthermore, the at least one solid electrolyte in step 3) is one or more of an oxide solid electrolyte, a sulfide solid electrolyte, a polymer solid electrolyte, and a halide solid electrolyte; Furthermore, the solid electrolyte is selected as an oxide solid electrolyte; preferably one or more of a garnet-type solid electrolyte, a perovskite-type solid electrolyte, and a sodium fast ion conductor-type solid electrolyte; Furthermore, the above-mentioned oxide solid electrolyte is selected to be a garnet-type solid electrolyte.
[0015] Furthermore, it is characterized in that: the mass of the metal salt in step 2) is 1-9% of the mass of the molten metal lithium.
[0016] Furthermore, the heating temperature in step 3) is 180-280°C.
[0017] Furthermore, the heating and the stirring are both performed under an inert gas atmosphere.
[0018] The second aspect of the present invention provides a composite lithium metal negative electrode, which is prepared by the preparation method of the composite lithium metal negative electrode as described above.
[0019] The third aspect of the present invention provides a solid-state battery, comprising a composite lithium metal negative electrode and a solid electrolyte, wherein the composite lithium metal negative electrode is the composite lithium metal negative electrode of the second aspect, and the solid electrolyte is the solid electrolyte of the first aspect.
[0020] Beneficial effects of the present invention: A simple and low-cost method is provided to prepare a composite lithium metal anode, which effectively improves the interfacial wettability between metallic lithium and garnet-type solid electrolyte and reduces the interfacial impedance; the composite lithium metal anode increases the lithium replenishment rate in the negative electrode bulk phase, eliminates lithium vacancies generated during lithium stripping at the negative electrode interface, inhibits the growth of lithium dendrites, and improves the dynamic stability of the interface during the solid-state battery cycle.
[0021] The present invention requires a small number of equipment, a simple preparation method and relatively simple raw materials, which can ensure the consistency of battery preparation and is easy to operate; the solid-state battery provided by the present invention has good cycle stability, high safety and good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] The present invention will be further described below in conjunction with the accompanying drawings.
[0023] Figure 1 This is a cycle performance diagram of a lithium symmetric battery assembled with a composite lithium metal electrode and a garnet-type solid electrolyte prepared in Example 3 at a current density of 1 mA cm-1; Figure 2 This is a long cycle performance diagram of a solid-state lithium metal battery assembled with a composite lithium metal negative electrode, a commercial lithium iron phosphate positive electrode and a garnet-type solid electrolyte prepared in Example 3 at a current density of 1 C; Figure 3 Schematic diagram of the composite lithium metal negative electrode of the present invention.
[0024] Figure numerals: 1. composite lithium metal negative electrode; 2. solid electrolyte. DETAILED DESCRIPTION
[0025] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] In order to further illustrate the present invention, the specific implementation of the present invention is further described below in conjunction with specific embodiments and drawings, but the implementation of the present invention is not limited thereto. Example 1
[0027] 1) In an inert environment, weigh 0.5 g of metallic lithium and place it on a stainless steel heating plate. Heat it at 240 °C until the metallic lithium melts into liquid metal balls. Use a stainless steel spatula and tweezers to carefully remove the impurity layer on the surface of the liquid lithium, leaking out fresh lithium metal liquid with a metallic luster.
[0028] 2) Weigh 5 mg of aluminum nitrate, the mass of which is 1% of the mass of lithium metal, mix it with molten lithium metal at 260 °C and stir it with a stainless steel spatula for 10 min to allow the aluminum nitrate and molten lithium metal to react fully. After naturally cooling to room temperature, a composite lithium metal negative electrode is obtained.
[0029] 3) Cover the surface of the garnet-type solid electrolyte sheet with the composite lithium metal obtained above, and heat the garnet-type solid electrolyte sheet covered with the composite lithium metal at 200 °C. After the composite lithium metal melts into liquid, gently apply it to the surface of the electrolyte sheet with tweezers, and assemble the battery after cooling. Perform the above treatment on both sides of the garnet electrolyte to assemble a lithium symmetrical battery. Use a garnet electrolyte sheet with a composite lithium metal on one side and a commercial lithium iron phosphate positive electrode sheet to assemble a lithium iron phosphate solid lithium metal battery. Example 2
[0030] The difference from Example 1 is that the mass of aluminum nitrate added in step 2) is 15 mg, and the mass of aluminum nitrate is 3% of the mass of lithium metal. Other than this, the other operating steps and conditions are the same as those in Example 1. Example 3
[0031] The difference from Example 1 is that the mass of aluminum nitrate added in step 2) is 25 mg, and the mass of aluminum nitrate is 5% of the mass of lithium metal. Other than this, the other operating steps and conditions are the same as those in Example 1. Example 4
[0032] The difference from Example 1 is that the mass of aluminum nitrate added in step 2) is 35 mg, and the mass of aluminum nitrate is 7% of the mass of lithium metal. Other than this, the other operating steps and conditions are the same as those in Example 1. Example 5
[0033] The difference from Example 1 is that the mass of aluminum nitrate added in step (2) is 45 mg, and the mass of aluminum nitrate is 9% of the mass of lithium metal. Other than this, the other operating steps and conditions are the same as those in Example 1. Comparative Example
[0034] The preparation method of the solid-state battery in this comparative example is basically the same as that in Example 1, except that: Lithium metal foil is directly covered on the two surfaces of the garnet-type solid electrolyte sheet to assemble into a lithium symmetrical battery. The above lithium symmetrical battery is then heated at 200 °C for 2 min and subjected to performance testing after cooling. Lithium iron phosphate solid-state lithium metal batteries are assembled using lithium metal as the negative electrode, a commercial lithium iron phosphate positive electrode sheet as the positive electrode, and garnet electrolyte as the electrolyte.
[0035] Table 1 Initial interfacial impedance of lithium symmetric batteries of different embodiments and their resistance at 1 mA cm -2 Cycling performance at current density Performance Testing The following performance tests were performed on the lithium symmetrical batteries and lithium iron phosphate solid-state lithium metal batteries in Examples 1-5 and Comparative Examples: The lithium symmetrical battery and lithium iron phosphate solid lithium metal battery in Examples 1-5 and Comparative Examples were subjected to cycle performance tests on a blue electric tester. -2 The lithium iron phosphate solid lithium metal battery was tested at a current density of 1 C under constant current charge and discharge test, and the test voltage range was 2.8-4.0 V. Table 1 and Table 2 are the electrochemical performance data of the lithium symmetric battery and the lithium iron phosphate solid lithium metal battery in Examples 1-5 of the present invention and the comparative example, respectively.
[0036] As shown in Table 1, the lithium symmetric batteries assembled with the composite lithium metal negative electrode and the garnet-type solid electrolyte prepared in Examples 1-5 all have low initial interface impedance. This is because the reaction between aluminum nitrate and molten lithium reduces the interface formation energy between lithium metal and electrolyte, improves the wettability of molten lithium to garnet electrolyte, and greatly reduces the interface impedance. -2 The cycle test was carried out at a high current density to evaluate the cycle performance of different composite lithium metal electrodes. The composite lithium metal negative electrode of Example 3 can be used at 1 mA cm -2 The stable cycling for 280 h at a high current density value of 1.5 Å indicates that the interface between the composite lithium metal and the electrolyte is very stable, and the ability to inhibit the growth of lithium dendrites has been enhanced. Unmodified molten lithium has a large surface tension and poor wettability with garnet. Therefore, the interface contact between the unmodified lithium metal and the garnet-type solid electrolyte is poor, resulting in a sharp increase in interface impedance. Lithium dendrites are very easy to form at high current density, so the lithium symmetric battery in the comparative example experiences a rapid short circuit.
[0037] As shown in Table 2, compared with the comparative example, the lithium iron phosphate solid-state lithium metal batteries assembled in Examples 1-5 show higher first-cycle discharge specific capacity and can run for more than 50 cycles. In particular, in Example 3, the battery has 157.2 mAh g -1 The high discharge specific capacity of the lithium iron phosphate solid-state lithium metal battery can be achieved at a high rate of 2 C with a capacity retention rate of 145.7 mAh g -1The battery of the comparative example cannot operate normally at a high current density of 1 C, indicating that the lithium iron phosphate solid-state battery assembled with the composite lithium metal negative electrode of the present invention has good performance.
[0038] Table 2 Cycling performance of lithium iron phosphate solid-state lithium metal batteries of different embodiments at 30 °C, 1 C <![CDATA[Initial discharge specific capacity (mAh g -1 ).]]> Capacity retention after 50 cycles (%) Capacity retention rate after 200 cycles (%) <![CDATA[Discharge specific capacity at 2C (mAh g -1 ).]]> Example 1 102.3 65 - - Example 2 135.3 85.1 32.5 65.2 Example 3 157.2 99.0 96.2 145.7 Example 4 144.6 77 21 32.1 Example 5 124.3 71 - - Comparative Example 89.2 - - - The above-described embodiments are merely methods for implementing the present disclosure, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the disclosed patents. It should be pointed out that any modifications, equivalent substitutions, improvements, etc. that can be made by a person of ordinary skill in the art without departing from the concept of the present disclosure should all be included in the protection scope of the present invention.
Claims
1. A method for preparing a composite lithium metal negative electrode, characterized in that: The method comprises the following steps: 1) heating and melting metallic lithium, and removing the impurity layer on the surface of the molten lithium solution to obtain molten metallic lithium; 2) adding at least one metal salt to the molten metal lithium obtained in step 1), heating, stirring evenly, reacting fully, and cooling to room temperature to obtain a composite lithium metal negative electrode; 3) Covering the composite lithium metal negative electrode obtained in step 2) on the surface of at least one solid electrolyte and performing a heating treatment; The metal salt is one or more of chloride metal salts, sulfate metal salts, carbonate metal salts, and nitrate metal salts, preferably a nitrate metal salt, and preferably the nitrate metal salt is one or more of sodium nitrate, potassium nitrate, lithium nitrate, ferric nitrate, ferrous nitrate, magnesium nitrate, aluminum nitrate, zinc nitrate, copper nitrate, bismuth nitrate, and tin nitrate.
2. The method for preparing a composite lithium metal negative electrode according to claim 1, characterized in that: In step 1), the heating temperature of the metallic lithium is 180-260°C.
3. The method for preparing a composite lithium metal negative electrode according to claim 1, characterized in that: The stirring time in step 2) is 2-20 min.
4. The method for preparing a composite lithium metal negative electrode according to claim 1, characterized in that: The heating temperature in step 2) is 220°C-280°C.
5. The method for preparing a composite lithium metal negative electrode according to claim 1, characterized in that: The mass of the metal salt in step 2) is 1-9% of the mass of the molten metal lithium.
6. The method for preparing a composite lithium metal negative electrode according to claim 1, characterized in that: The solid electrolyte in step 3) is one or more of an oxide solid electrolyte, a sulfide solid electrolyte, a polymer solid electrolyte, and a halide solid electrolyte, preferably an oxide solid electrolyte, and the oxide solid electrolyte is one or more of a garnet-type solid electrolyte, a perovskite-type solid electrolyte, and a sodium fast ion conductor-type solid electrolyte.
7. The method for preparing a composite lithium metal negative electrode according to claim 1, characterized in that: The heating temperature in step 3) is 180-280°C.
8. The method for preparing a composite lithium metal negative electrode according to claim 1, characterized in that: The heating and the stirring are both performed under an inert gas atmosphere.
9. A composite lithium metal negative electrode, characterized in that: The composite lithium metal negative electrode is prepared by the preparation method of any one of claims 1 to 8.
10. A solid-state battery, characterized in that: It comprises a composite lithium metal negative electrode and a solid electrolyte, wherein the composite lithium metal negative electrode is the composite lithium metal negative electrode according to claim 9, and the solid electrolyte is the solid electrolyte according to claim 6.
Citation Information
Patent Citations
Composite lithium and solid-state lithium battery
CN114335494A
Composite lithium metal negative electrode material, preparation method thereof and metal lithium battery
CN114665098A
Composite lithium negative electrode material as well as preparation method and application thereof
CN117410484A
Solid electrolyte-lithium negative electrode interface modification method
CN117976997A
Preparation method of surface-modified lithium metal negative electrode, lithium metal negative electrode, and lithium metal battery
WO2024164690A1