Positive electrode material and preparation method thereof, positive plate and lithium ion battery
By using a composite material with a core-shell structure in the positive electrode material of lithium-ion battery and covering the carbon layer, the processing problems of the material during the homogenization process are solved, the energy density and circulation performance of the battery are improved, and high-gauge capacity and excellent cycling performance.
Patent Information
- Application Number
- CN202411344105.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-11-29
AI Technical Summary
During the homogenization process, the existing lithium-ion battery positive electrode materials have high residual alkali content, which leads to a rapid rebound in the slurry viscosity, easily forming gels, and cannot be processed, and the energy density and cycle life are insufficiently improved.
The composite material with a core-shell structure is adopted. The core is lithium lithium ferrate rich, and the shell is lithium iron phosphate material. The surface is covered with carbon coating. It is prepared by hydrothermal reaction and electron beam evaporation to control the core-shell structure. Mass ratio and thickness of the carbon cladding to improve the gram capacity and cycling performance of the material.
The processability and high energy density of the positive electrode material are achieved, which significantly improves the circulation performance of the battery, avoids processing problems, and improves the conductivity and stability of the material.
Smart Images

Figure CN119050326A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a positive electrode material and a preparation method thereof, a positive electrode sheet and a lithium ion battery. Background Art
[0002] In recent years, with the gradual depletion of traditional fossil energy and the increasingly serious environmental degradation caused by the use of fossil energy, the research and development of new renewable green clean energy is particularly important. However, renewable energy such as wind energy, solar energy, and tidal energy are discontinuous, and if you want to make better use of them, you need to develop supporting energy storage devices.
[0003] Lithium-ion batteries have become a type of energy storage secondary battery with broad application prospects due to their advantages such as high discharge voltage, high specific energy density, long cycle life, and wide applicable temperature range.
[0004] At present, both lithium iron phosphate batteries and ternary batteries have the demand for improved energy density and cycle life. Pre-lithium technology is an effective way to meet this demand. Positive electrode pre-lithium is the most commonly used and safest pre-lithium technology. The positive electrode lithium supplements that have reached commercialization mainly include lithium-rich lithium iron oxide and lithium-rich lithium nickel oxide. Among them, lithium-rich lithium iron oxide has a higher lithium supplement efficiency and more cost advantages. However, directly mixing the lithium supplement into the positive electrode slurry will cause a series of processing problems. During the homogenization process, due to the high residual alkali content of the material, the slurry viscosity rebounds quickly and gels easily, which ultimately makes it impossible to process.
[0005] Therefore, it is of great significance to provide a product or method that can significantly increase the gram capacity of the material by replenishing lithium while avoiding processing problems.
[0006] In view of this, the present invention is proposed. Summary of the invention
[0007] The first object of the present invention is to provide a positive electrode material that is easy to process and can significantly increase the energy density of the battery and improve the cycle performance of the battery. The gram capacity of the material is significantly increased by lithium supplementation, while avoiding processing problems.
[0008] The second object of the present invention is to provide a method for preparing a positive electrode material, wherein the positive electrode material prepared by the method has the advantages of good processing performance, high specific capacity, and good cycle performance.
[0009] The third object of the present invention is to provide a positive electrode sheet having the advantages of high gram capacity and good cycle performance.
[0010] A fourth object of the present invention is to provide a lithium ion battery having high specific capacity and excellent cycle performance.
[0011] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0012] The present invention first provides a positive electrode material, including a composite material with a core-shell structure, wherein the core of the core-shell structure includes lithium-rich lithium ferrite, and the shell of the core-shell structure includes a lithium iron phosphate material; at least part of the surface of the composite material is partially or completely coated with a carbon coating layer.
[0013] Furthermore, the mass ratio of the core to the shell of the core-shell structure is 0.01-0.08:1.
[0014] Furthermore, the thickness of the carbon coating layer is 1 to 10 nm.
[0015] Furthermore, the mass ratio of the carbon coating layer to the composite material is 0.5-3:97-99.5.
[0016] Furthermore, the chemical formula of the lithium iron phosphate material is LiFe 1-x M x PO4, wherein 0≤x<0.01, and M includes at least one of Ti, Zr, V, La and Sr elements.
[0017] The present invention further provides a method for preparing the positive electrode material, comprising the following steps: (a) mixing lithium-rich lithium ferrite with a lithium source, an iron source, a phosphorus source and water and subjecting the mixture to a hydrothermal reaction, and after the hydrothermal reaction is completed, performing solid-liquid separation to obtain a precursor; sintering the precursor to obtain a composite material having a core-shell structure; (b) making the composite material into a composite material film, and using the composite material film as a substrate and a polymer carbon source as an evaporation target, using an electron beam evaporation method to grow a polymer layer on the substrate, and then calcining.
[0018] Furthermore, in step (a), a dopant containing M is added during the mixing process, wherein M includes at least one of the elements Ti, Zr, V, La and Sr.
[0019] Furthermore, in step (a), the temperature of the hydrothermal reaction is 200-300°C.
[0020] Furthermore, in step (a), the hydrothermal reaction time is 8 to 12 hours.
[0021] Furthermore, in step (a), the sintering temperature is 700-800°C.
[0022] Furthermore, in step (a), the sintering holding time is 5 to 10 hours.
[0023] Furthermore, in step (a), the sintering atmosphere includes an inert atmosphere.
[0024] Furthermore, in step (a), the particle size Dv50 of the composite material is 1 to 3 μm.
[0025] Furthermore, in step (a), the particle size Dv50 of the lithium-rich lithium ferrite is 100 to 300 nm.
[0026] Furthermore, in step (a), the preparation method of the lithium-rich lithium iron oxide comprises: mixing a lithium source, an iron source and water, and conducting a hydrothermal reaction at 150 to 300° C. for 5 to 12 hours, then performing solid-liquid separation, washing and drying to obtain a solid powder, and heat treating the solid powder at 700 to 800° C. for 3 to 8 hours in an inert atmosphere to obtain the lithium-rich lithium iron oxide.
[0027] Furthermore, in step (b), the method for preparing the composite material film comprises: mixing the composite material with a solvent to obtain a slurry; coating the slurry on a substrate, and drying to obtain a composite material film.
[0028] Furthermore, in step (b), the solvent includes at least one of NMP, anhydrous ethanol and isopropanol.
[0029] Furthermore, in step (b), after the composite material and the solvent are mixed, ball milling is performed.
[0030] Furthermore, in step (b), the solid content of the slurry is 40% to 50%.
[0031] Furthermore, in step (b), the coating method includes spin coating; the spin coating method includes: dropping the slurry on the substrate, letting it stand for 3 to 10 minutes, and then centrifuging at a rate of 1800 to 2300 r / min for 5 to 15 seconds to perform the spin coating; the number of spin coating is 1 to 3 times.
[0032] Furthermore, in step (b), the coating is performed until the thickness of the obtained film is 5 to 10 μm, and then the drying is performed.
[0033] Furthermore, in step (b), the drying temperature is 80-100° C. and the drying time is 2-5 hours.
[0034] Furthermore, in step (b), the polymer carbon source includes at least one of glucose, polyvinyl alcohol and polyethylene glycol.
[0035] Furthermore, in step (b), the thickness of the polymer layer is 1 to 5 nm.
[0036] Furthermore, in step (b), the calcination temperature is 300-500°C.
[0037] Furthermore, in step (b), the calcination time is 3 to 8 hours.
[0038] Furthermore, in step (b), the calcination atmosphere includes an inert atmosphere.
[0039] Furthermore, after step (b), the following steps are also included: (c) crushing the carbon-containing composite layer obtained after calcination in step (b), then making it into a film and growing a polymer layer on its surface, and then calcining it; repeating step (c) at least 3 times; wherein the material is crushed to a particle size Dv50 of 0.5 to 2 μm.
[0040] The present invention further provides a positive electrode sheet, comprising the positive electrode material, or the positive electrode material prepared by the preparation method of the positive electrode material.
[0041] The present invention also provides a lithium ion battery, comprising the positive electrode sheet.
[0042] Compared with the prior art, the present invention has the following beneficial effects:
[0043] The positive electrode material provided by the present invention is easy to process and can effectively increase the gram capacity of the battery and improve the cycle performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0045] Figure 1 A schematic diagram of the structure of the positive electrode material when the carbon coating layer provided by the present invention completely covers the composite material;
[0046] Figure 2 A comparison chart of the cycle test results of the soft-pack batteries of Example 1 and Comparative Example 1 provided by the present invention. DETAILED DESCRIPTION
[0047] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but it will be understood by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0048] If there is no special explanation, in the present invention, "the first aspect", "the second aspect", "the third aspect", "the fourth aspect", etc. are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "the first", "the second", "the third", "the fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.
[0049] If there is no special explanation, the "include" and "comprising" mentioned in the present invention represent open-ended or closed-ended expressions. For example, the "include" and "comprising" may represent that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0050] If there is no special explanation, in the present invention, "one or more" or "at least one" refers to any one, any two or more of the listed items. Among them, "several" refers to any two or more of the listed items.
[0051] In a first aspect, the present invention provides a positive electrode material, which includes a composite material having a core-shell structure, wherein the core of the core-shell structure includes lithium-rich ferrite, and the shell of the core-shell structure includes a lithium iron phosphate material. That is, the main component of the core of the composite material includes lithium-rich ferrite, and the chemical formula of lithium-rich ferrite is Li5FeO4 (abbreviated as LFO); the main component of the shell of the composite material includes lithium iron phosphate material (abbreviated as LFP). The lithium iron phosphate material includes doped lithium iron phosphate and / or undoped lithium iron phosphate.
[0052] At least part of the surface of the composite material is partially or completely coated with a carbon coating layer. That is, at least part of the surface of the composite material has a carbon coating layer, and the carbon coating layer partially or completely coats (covers) the composite material.
[0053] like Figure 1The structure diagram of the positive electrode material is shown when the carbon coating layer completely covers the composite material. The core of the composite material with a core-shell structure is marked as LFO core, and the shell of the composite material with a core-shell structure is marked as LFP inner shell.
[0054] The positive electrode material provided by the present invention is easy to process and can significantly increase the energy density of the battery and improve the cycle performance of the battery. The gram capacity of the material is significantly increased by lithium supplementation and processing problems are avoided.
[0055] Specifically, lithium iron oxide (LiFePO4) mainly plays a role in replenishing lithium. Lithium iron phosphate (LiFePO4) materials can provide reversible capacity. The carbon coating layer can improve the conductivity of the material and inhibit the growth of the grains of the material.
[0056] In some specific embodiments, the mass ratio of the core to the shell of the core-shell structure is 0.01 to 0.08:1, including but not limited to any point value of 0.01:1, 0.02:1, 0.03:1, 0.04:1, 0.05:1, 0.06:1, 0.07:1, 0.08:1 or any range value between two of them. Controlling the mass ratio range can improve both capacity and cycle performance.
[0057] In some specific embodiments, the thickness of the carbon coating layer is 1 to 10 nm, including but not limited to any point value of 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, and 10 nm, or a range value between any two of them; preferably 2 to 5 nm.
[0058] In some specific embodiments, the mass ratio of the carbon coating layer to the composite material is 0.5-3:97-99.5, including but not limited to 0.5:97, 0.5:98, 0.5:99, 0.8:97, 0.8:98, 0.8:99, 1:97, 1:97.5, 1:98, 1:98.5, 1:99, 1:99.5, 2:97, 2:98, 2:99, 3:97, 3:98, 3:99, any one of the point values or the range values between any two of them.
[0059] In some specific embodiments, the chemical formula of the lithium iron phosphate material is LiFe 1-x M xPO4 (abbreviated as LFP). Wherein, 0≤x<0.01, including but not limited to any point value of 0, 0.001, 0.002, 0.003, 0.004, 0.005, 0.006, 0.007, 0.008, 0.009, 0.01 or any range value between two of them; M is a doping element, M includes at least one of Ti, Zr, V, La and Sr elements, preferably at least two or more than three. Doping M is beneficial to further improve the capacity and cycle performance of the positive electrode material.
[0060] In some specific embodiments, the LFO is prepared by a hydrothermal method. The LFO prepared by the hydrothermal method has better uniformity of distribution of various elements therein, high cleanliness after subsequent sintering, and high material capacity.
[0061] In some specific embodiments, the composite material with a core-shell structure is prepared by a hydrothermal method.
[0062] In some specific embodiments, the carbon coating layer is prepared by electron beam evaporation. The carbon coating layer prepared by this method has a high bonding force with the composite material, and the carbon coating is denser, the conductivity of the positive electrode material is good, and the polarization is small.
[0063] In a second aspect, the present invention provides a method for preparing the above-mentioned positive electrode material, comprising the following steps:
[0064] (a) Weigh each raw material according to the target ratio, mix the lithium-rich lithium ferrite with a lithium source, an iron source, a phosphorus source and water, and perform a hydrothermal reaction. After the hydrothermal reaction is completed, separate the solid and liquid, wash and dry to obtain a precursor. The precursor is sintered and then cooled to obtain a composite material with a core-shell structure. Optionally (optional or not), a dopant containing M is also added during the above mixing process, wherein M includes at least one of the elements Ti, Zr, V, La and Sr. Among them, sintering can improve the crystallinity of the material, make the material structure more stable, the capacity is higher, and the cycle performance is better.
[0065] The core of the composite material with a core-shell structure includes lithium-rich lithium ferrite, and the shell includes lithium iron phosphate material.
[0066] (b) The composite material is made into a composite film, that is, the granular composite material is made into a film. Then, the composite film is used as a substrate, and the polymer carbon source (i.e., carbon-containing polymer) is used as an evaporation target. The polymer layer is grown on the surface of the substrate by electron beam evaporation, and then calcined. It can be understood that the main component of the polymer layer is a carbon-containing polymer, and the carbon-containing polymer reacts to generate amorphous carbon during calcination. Amorphous carbon is coated on the surface of a portion of the composite material having a core-shell structure, which is the positive electrode material.
[0067] The positive electrode material prepared by the preparation method of the positive electrode material provided by the present invention has excellent processing performance, high material specific capacity, and significantly improved cycle performance.
[0068] In some specific embodiments, in step (a), a dopant containing M is added during the mixing process, wherein M includes at least one of Ti, Zr, V, La and Sr elements.
[0069] In some specific embodiments, in step (a), the temperature of the hydrothermal reaction is 200-300°C, including but not limited to any point value of 200°C, 220°C, 230°C, 250°C, 270°C, 280°C, 300°C or a range between any two of them.
[0070] In some specific embodiments, in step (a), the hydrothermal reaction time is 8 to 12 hours, including but not limited to any one of 8 hours, 9 hours, 10 hours, 11 hours, and 12 hours, or a range between any two of them.
[0071] In some specific embodiments, in step (a), the sintering temperature is 700-800°C, including but not limited to any point value of 700°C, 720°C, 730°C, 750°C, 780°C, 800°C or a range between any two of them.
[0072] In some specific embodiments, in step (a), the sintering holding time is 5 to 10 hours, including but not limited to any one of 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, and 10 hours, or a range between any two of them.
[0073] In some specific embodiments, in step (a), the sintering atmosphere includes an inert atmosphere; wherein the inert atmosphere includes a nitrogen atmosphere or an argon atmosphere, but is not limited thereto.
[0074] In some specific embodiments, in step (a), the particle size Dv50 of the composite material is 1 to 3 μm, including but not limited to any point value of 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm or a range value between any two of them; preferably 2 to 3 μm.
[0075] In some specific embodiments, in step (a), the molar ratio of Li:Fe:M:P is 1:1-x:x:1, wherein x=0-0.01, preferably x=0.001-0.01; the corresponding masses of lithium source, iron source, dopant containing M and phosphorus source are weighed. The lithium source includes any soluble lithium-containing compound commonly used in the art, such as lithium hydroxide, lithium carbonate, etc., the iron source includes any soluble iron-containing compound commonly used in the art, such as ferrous sulfate, ferrous chloride, ferric sulfate or ferric chloride, etc., the dopant containing M includes nitrate containing M, and the phosphorus source includes phosphoric acid, ammonium phosphate or sodium phosphate, etc., but is not limited thereto.
[0076] In some specific embodiments, in step (a), the particle size Dv50 of the lithium-rich lithium ferrite is 100-300 nm, including but not limited to any point value of 100 nm, 150 nm, 200 nm, 250 nm, 300 nm or a range value between any two of them; preferably 150-250 nm.
[0077] In some specific embodiments, in step (a), the preparation method of the lithium-rich lithium iron oxide comprises: mixing a lithium source, an iron source and water, and performing a hydrothermal reaction at 150 to 300° C. for 5 to 12 hours, and after the reaction is completed, performing solid-liquid separation, washing and drying to obtain a solid powder, and heat treating the solid powder at 700 to 800° C. for 3 to 8 hours in an inert atmosphere to obtain the lithium-rich lithium iron oxide. The inert atmosphere is, for example, a nitrogen atmosphere or an argon atmosphere, but is not limited thereto. The temperature of the hydrothermal reaction includes but is not limited to any point value of 150°C, 180°C, 200°C, 230°C, 250°C, 270°C, 300°C or any range value between the two; the time of the hydrothermal reaction includes but is not limited to any point value of 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h or any range value between the two; the temperature of the heat treatment includes but is not limited to any point value of 700°C, 720°C, 730°C, 750°C, 780°C, 800°C or any range value between the two; the time of the heat treatment includes but is not limited to any point value of 3h, 4h, 5h, 6h, 7h, 8h or any range value between the two. According to the molar ratio of Li:Fe of 5:1, the corresponding mass of lithium source and iron source are weighed, wherein the lithium source includes any soluble lithium-containing compound commonly used in the art, such as lithium hydroxide or lithium carbonate, and the iron source includes any soluble iron-containing compound commonly used in the art, such as ferric nitrate, but not limited thereto.
[0078] In some specific embodiments, in step (b), the method for preparing the composite material film comprises the following steps: mixing the composite material with a solvent to obtain a slurry, coating the slurry on a substrate, and drying to obtain a composite material film.
[0079] In some specific embodiments, in step (b), the solvent includes at least one of NMP (N-methylpyrrolidone), anhydrous ethanol, and isopropanol.
[0080] In some specific embodiments, in step (b), after the composite material and the solvent are mixed, ball milling is performed. Ball milling can reduce the primary particle size of the material, which is beneficial to the material capacity.
[0081] In some specific embodiments, in step (b), the solid content of the slurry is 40% to 50%, including but not limited to any point value of 40%, 41%, 43%, 45%, 46%, 48%, 50% or a range value between any two of them.
[0082] In some specific embodiments, in step (b), the coating method includes spin coating, but is not limited thereto.
[0083] In some specific embodiments, in step (b), the spin coating device includes a spin coater.
[0084] In some specific embodiments, in step (b), the spin coating method comprises the following steps: dropping the slurry on the substrate, letting it stand for 3 to 10 minutes (including but not limited to any one of 3 minutes, 4 minutes, 5 minutes, 6 minutes, 8 minutes, and 10 minutes, or any range between two of them), and then centrifuging at a rate of 1800 to 2300 r / min (including but not limited to any one of 1800 r / min, 1900 r / min, 2000 r / min, 2100 r / min, 2200 r / min, and 2300 r / min, or any range between two of them) for 5 to 15 seconds (including but not limited to any one of 5 seconds, 6 seconds, 7 seconds, 8 seconds, 10 seconds, 12 seconds, 13 seconds, and 15 seconds, or any range between two of them) to perform the spin coating. Preferably, the spin coating is performed 1 to 3 times (including but not limited to any one of 1, 2, and 3 times or a range between any two of them), that is, the spin coating is repeated 1 to 3 times according to the above steps and parameters.
[0085] In some specific embodiments, in step (b), the substrate includes but is not limited to a titanium substrate.
[0086] In some specific embodiments, in step (b), the method of making the composite material into a composite material film specifically includes: fixing a titanium substrate on a centrifuge of a spin coater, slowly adding the composite material with a core-shell structure into a solvent under ultrasonic conditions, and ball milling to obtain a slurry; dropping the slurry on a titanium substrate, letting it stand for 3 to 10 minutes, centrifuging at a rate of 1800 to 2300 r / min for 5 to 15 seconds, repeating the spin coating 1 to 3 times to obtain a wet film with a thickness of 5 to 10 μm, and drying the wet film to obtain a composite material film.
[0087] In some specific embodiments, in step (b), the coating is performed to obtain a film with a thickness of 5 to 10 μm, including but not limited to any point value of 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm or a range value between any two of them, and then the drying is performed.
[0088] In some specific embodiments, in step (b), the drying temperature is 80-100°C, including but not limited to any one of 80°C, 85°C, 90°C, 95°C, and 100°C, or a range between any two of them; the drying time is 2-5h, including but not limited to any one of 2h, 3h, 4h, and 5h, or a range between any two of them.
[0089] In some specific embodiments, in step (b), the polymer carbon source includes at least one of glucose, polyvinyl alcohol, and polyethylene glycol.
[0090] In some specific embodiments, in step (b), the thickness of the polymer layer is 1 to 5 nm, including but not limited to any point value of 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, or a range value between any two of them.
[0091] In some specific embodiments, in step (b), the calcination temperature is 300-500°C, including but not limited to any one of 300°C, 350°C, 400°C, 450°C, 500°C or a range between any two of them.
[0092] In some specific embodiments, in step (b), the calcination time is 3 to 8 hours, including but not limited to any one of 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, and 8 hours, or a range between any two of them.
[0093] In some specific embodiments, in step (b), the calcination atmosphere includes an inert atmosphere, such as a nitrogen atmosphere or an argon atmosphere, but is not limited thereto.
[0094] After the calcination in step (b), a carbon-containing composite layer is obtained. In some specific embodiments, after step (b), the following step (c) is further included: (c) the carbon-containing composite layer obtained after the calcination in step (b) is crushed, then made into a film and a polymer layer is grown on its surface, and then calcined. Step (c) is repeated at least 3 times, and can also be repeated four times, five times, six times, eight times or ten times.
[0095] The particle size Dv50 of the crushed material is 0.5 to 2 μm, including but not limited to any point value of 0.5 μm, 0.6 μm, 0.8 μm, 1 μm, 1.3 μm, 1.5 μm, 1.8 μm, 2 μm or a range value between any two of them.
[0096] Repeating the film and growing the polymer layer multiple times is conducive to promoting more carbon coating layers on the surface of the composite material with a core-shell structure. After repeating the above operation several times, the surface of each composite material can be coated with a complete carbon coating layer. This is conducive to improving the conductivity of the positive electrode material.
[0097] In some specific embodiments, the operation method and parameters for forming the thin film in step (c) are the same as those for preparing the composite material film in step (b), the operation method and parameters for growing the polymer layer in step (c) are the same as those for growing the polymer layer by electron beam evaporation in step (b), and the calcination method and parameters in step (c) are the same as those in step (b), which will not be repeated here.
[0098] In a third aspect, the present invention provides a positive electrode sheet, comprising the above-mentioned positive electrode material, or the positive electrode material prepared according to the above-mentioned method for preparing the positive electrode material.
[0099] The positive electrode sheet has the advantages of high gram capacity and good cycle performance.
[0100] Optionally, the positive electrode sheet further includes a binder and / or a conductive agent, which is not limited in the present invention.
[0101] In a fourth aspect, the present invention provides a lithium-ion battery comprising the above-mentioned positive electrode sheet.
[0102] The lithium-ion battery has high gram capacity and excellent cycle performance.
[0103] Optionally, the lithium-ion battery further comprises a negative electrode sheet, a separator and an electrolyte, which is not limited in the present invention.
[0104] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.
[0105] Example 1
[0106] The method for preparing the positive electrode material provided in this embodiment comprises the following steps:
[0107] (1) According to the molar ratio of Li:Fe of 5:1, lithium hydroxide and ferric nitrate of corresponding mass are weighed and dissolved in a reactor, and a hydrothermal reaction is carried out at 200°C for 8 hours, and then LFO powder is obtained through filtering, washing and drying steps. The obtained LFO powder is sintered at 800°C in a nitrogen atmosphere for 5 hours to obtain LFO nanocrystalline particles (i.e., lithium iron-rich lithium), and the particle size Dv50 of the particles is 150 nm.
[0108] (2) The LFO nanocrystalline particles obtained in step (1) are placed in a reactor containing water, and corresponding masses of lithium carbonate, ferrous sulfate, V2O5, La(NO3)3 and sodium phosphate are weighed and dissolved in the reactor according to the molar ratio of Li:Fe:V:La:P of 1:0.994:0.004:0.002:1, wherein the mass ratio of the theoretical yield (mass) of lithium iron phosphate material to the mass of LFO nanocrystalline particles is 94:5, and then a hydrothermal reaction is carried out at 260°C for 10 hours, and then a core-shell structure precursor is obtained by filtering, washing and drying, and then the precursor is sintered at 780°C for 10 hours (nitrogen atmosphere) to obtain composite material crystal particles with a core-shell structure, and the particle size Dv50 of the particles is 2 μm.
[0109] (3) Fixing the titanium substrate (base) on the centrifuge of the spin coater, slowly adding the composite material with a core-shell structure obtained in step (2) into the solvent NMP under ultrasonic conditions, and performing ball milling to obtain a slurry with a solid content of 45%; dropping the slurry on the titanium substrate, letting it stand for 5 minutes, centrifuging it at a rate of 2000 r / min for 10 seconds, and spin coating it twice to obtain a wet film with a thickness of 8 μm, heat treating (drying) the wet film at 100° C. for 3 hours, peeling off the substrate, and obtaining an LFP / LFO composite film.
[0110] (4) Using a composite polymer carbon source of polyvinyl alcohol and polyethylene glycol in a mass ratio of 1:1 as an evaporation target, the LFP / LFO composite film prepared in step (3) is used as a substrate, and a polyvinyl alcohol / polyethylene glycol film (i.e., a polymer layer) is grown on the substrate by electron beam evaporation until the thickness of the polyvinyl alcohol / polyethylene glycol film is 1 nm, and then it is calcined at 400° C. for 5 h under high-purity nitrogen.
[0111] (5) The calcined double-layer film material is removed, ground and crushed to a Dv50 of 1.0 μm, and then the crushed material is made into a film, and a polymer layer is grown on the surface of the film, and then calcined. This is repeated 3 times to obtain the final positive electrode material. In this step (5): the operation method and parameters for preparing the film are the same as those for preparing the LFP / LFO composite film in step (3) of Example 1, the operation method and parameters for growing the polymer layer are the same as those for growing the polymer layer by electron beam evaporation in step (4) of Example 1, and the calcination method and parameters are the same as those for calcining in step (4) of Example 1, which will not be described in detail.
[0112] The positive electrode material provided in this embodiment includes a composite material with a core-shell structure, wherein the core of the core-shell structure includes lithium-rich lithium iron oxide (Li5FeO4), and the shell of the core-shell structure includes a lithium iron phosphate material, and the chemical formula of the lithium iron phosphate material is LiFe 0.994 V 0.004 La 0.002 PO4. The surface of the composite material is coated with a complete carbon coating layer. Among them, the mass ratio of lithium iron-rich lithium ferrate, lithium iron phosphate material and carbon coating layer is 5:94:1. That is, the mass ratio of the core to the shell of the core-shell structure is 0.053:1, and the mass ratio of the carbon coating layer to the composite material with the core-shell structure is 1:99. The thickness of the carbon coating layer is 3nm.
[0113] Example 2
[0114] The preparation method of the positive electrode material provided in this embodiment is basically the same as that in Embodiment 1, except that, in step (2), corresponding masses of lithium hydroxide, ferrous sulfate, V2O5, strontium nitrate and sodium phosphate are weighed according to the molar ratio of Li:Fe:V:Sr:P of 1:0.994:0.003:0.003:1.
[0115] The chemical formula of the lithium iron phosphate material in the positive electrode material prepared in this embodiment is LiFe 0.994 V 0.003 Sr 0.003 PO4.
[0116] Example 3
[0117] The preparation method of the positive electrode material provided in this embodiment is basically the same as that in embodiment 1, except that, in step (2), lithium hydroxide, ferrous sulfate, titanium tetrachloride, zirconium nitrate and sodium phosphate of corresponding mass are weighed according to the molar ratio of Li:Fe:Ti:Zr:P of 1:0.994:0.004:0.002:1. That is, the chemical formula of the lithium iron phosphate material in the positive electrode material prepared in this embodiment is LiFe 0.994 Ti 0.004 Zr 0.002 PO4.
[0118] Example 4
[0119] The preparation method of the positive electrode material provided in this embodiment is basically the same as that in Example 1, except that in step (2), the mass ratio of the theoretical yield (mass) of the lithium iron phosphate material to the mass ratio of the LFO nanocrystal particles is 96:3. That is, the mass ratio of the core to the shell of the composite material with a core-shell structure in the positive electrode material prepared in this embodiment is 0.031:1.
[0120] Example 5
[0121] The preparation method of the positive electrode material provided in this embodiment is basically the same as that in Example 1, except that in step (2), the mass ratio of the theoretical yield (mass) of the lithium iron phosphate material to the mass ratio of the LFO nanocrystal particles is 93:6. That is, the mass ratio of the core to the shell of the composite material with a core-shell structure in the positive electrode material prepared in this embodiment is 0.065:1.
[0122] Example 6
[0123] The method for preparing the positive electrode material provided in this embodiment comprises the following steps:
[0124] (1) According to the molar ratio of Li:Fe of 5:1, lithium hydroxide and ferric nitrate of corresponding mass are weighed and dissolved in a reactor, and a hydrothermal reaction is carried out at 300°C for 12 hours, and then LFO powder is obtained through filtering, washing and drying steps. The obtained LFO powder is sintered at 700°C in a nitrogen atmosphere for 8 hours to obtain LFO nanocrystalline particles (i.e., lithium iron-rich lithium), and the particle size Dv50 of the particles is 250 nm.
[0125] (2) The LFO nanocrystalline particles obtained in step (1) are placed in a reactor containing water, and corresponding masses of lithium carbonate, ferrous sulfate, V2O5, La(NO3)3 and sodium phosphate are weighed and dissolved in the reactor according to the molar ratio of Li:Fe:V:La:P of 1:0.994:0.004:0.002:1, wherein the mass ratio of the theoretical yield (mass) of lithium iron phosphate material to the mass of LFO nanocrystalline particles is 94:5, and then a hydrothermal reaction is carried out at 200°C for 12 hours, and then a core-shell structure precursor is obtained by filtering, washing and drying, and then the precursor is sintered at 700°C for 6 hours (nitrogen atmosphere) to obtain composite material crystal particles with a core-shell structure, and the particle size Dv50 of the particles is 3 μm.
[0126] (3) Fixing the titanium substrate (base) on the centrifuge of the spin coater, slowly adding the composite material with a core-shell structure obtained in step (2) into the solvent anhydrous ethanol under ultrasonic conditions, and performing ball milling to obtain a slurry with a solid content of 50%; dropping the slurry on the titanium substrate, letting it stand for 10 minutes, centrifuging it at a speed of 2300 r / min for 10 seconds, and spin coating it for 3 times to obtain a wet film with a thickness of 10 μm, heat treating (drying) the wet film at 80° C. for 5 hours, peeling off the substrate, and obtaining an LFP / LFO composite film.
[0127] (4) Using a composite polymer carbon source of polyvinyl alcohol and polyethylene glycol in a mass ratio of 2:1 as an evaporation target, the LFP / LFO composite film prepared in step (3) is used as a substrate, and a polyvinyl alcohol / glucose film (i.e., a polymer layer) is grown on the substrate by electron beam evaporation until the thickness of the polyvinyl alcohol / glucose film is 1 nm, and then calcined at 500° C. for 6 h under high-purity nitrogen.
[0128] (5) The calcined double-layer film material is removed, ground and crushed to a Dv50 of 1.0 μm, and then the crushed material is made into a film, and a polymer layer is grown on the surface of the film, and then calcined. This is repeated 3 times to obtain the final positive electrode material. In this step (5): the operation method and parameters for preparing the film are the same as those for preparing the LFP / LFO composite film in step (3) of Example 1, the operation method and parameters for growing the polymer layer are the same as those for growing the polymer layer by electron beam evaporation in step (4) of Example 1, and the calcination method and parameters are the same as those for calcining in step (4) of Example 1, which will not be described in detail.
[0129] The positive electrode material provided in this embodiment includes a composite material with a core-shell structure, wherein the core of the core-shell structure includes lithium-rich lithium iron oxide (Li5FeO4), and the shell of the core-shell structure includes a lithium iron phosphate material, and the chemical formula of the lithium iron phosphate material is LiFe 0.994 V 0.004 La 0.002PO4. The surface of the composite material is coated with a complete carbon coating layer. Among them, the mass ratio of lithium iron-rich lithium ferrate, lithium iron phosphate material and carbon coating layer is 5:94:1. That is, the mass ratio of the core to the shell of the core-shell structure is 0.053:1, and the mass ratio of the carbon coating layer to the composite material with the core-shell structure is 1:99. The thickness of the carbon coating layer is 3nm.
[0130] Example 7
[0131] The method for preparing the positive electrode material provided in this embodiment comprises the following steps:
[0132] Steps (1) to (4): Same as steps (1) to (4) in Example 1.
[0133] (5) Grind and crush the calcined double-layer film material obtained in step (4) to a particle size Dv50 of 2.0 μm, then make the crushed material into a film, grow a polymer layer on the surface of the film, and then calcine, repeat 3 times in total, and obtain the final positive electrode material. In this step (5): the operation method and parameters for preparing the film are the same as those for preparing the LFP / LFO composite film in step (3) of Example 1, the operation method and parameters for growing the polymer layer are the same as those for growing the polymer layer by electron beam evaporation in step (4) of Example 1, and the calcination method and parameters are the same as those for calcining in step (4) of Example 1, which will not be repeated.
[0134] In the positive electrode material provided in this embodiment, the mass ratio of lithium iron-rich lithium ferrate, lithium iron phosphate material and carbon coating layer is 5:94:1. That is, the mass ratio of carbon coating layer to the composite material with core-shell structure is 1:99. The thickness of carbon coating layer is 3nm.
[0135] Example 8
[0136] The method for preparing the positive electrode material provided in this embodiment comprises the following steps:
[0137] Steps (1) to (4): Same as steps (1) to (4) in Example 1.
[0138] (5) Grind and crush the calcined double-layer film material obtained in step (4) to a particle size Dv50 of 1.0 μm, then make the crushed material into a film, grow a polymer layer on the surface of the film, and then calcine, repeat 6 times in total, and obtain the final positive electrode material. In this step (5): the operation method and parameters for preparing the film are the same as those for preparing the LFP / LFO composite film in step (3) of Example 1, the operation method and parameters for growing the polymer layer are the same as those for growing the polymer layer by electron beam evaporation in step (4) of Example 1, and the calcination method and parameters are the same as those for calcining in step (4) of Example 1, which will not be repeated.
[0139] In the positive electrode material provided in this embodiment, the mass ratio of lithium-rich lithium iron oxide, lithium iron phosphate material and carbon coating layer is 5:94:2. That is, the mass ratio of carbon coating layer to the composite material with core-shell structure is 2:99. The thickness of carbon coating layer is 6nm.
[0140] Comparative Example 1
[0141] The preparation method of the positive electrode material provided in this comparative example is a solid phase method, which specifically includes the following steps: according to the molar ratio of Li:Fe of 1:1, corresponding masses of lithium carbonate and iron phosphate are weighed and placed in a ball mill, and then a glucose carbon source is placed in the ball mill, and ball milled with water as a medium for 5 hours, and then dried in an oven at 100°C, and then the obtained mixture powder is sintered at 780°C in a nitrogen atmosphere for 10 hours to obtain a solid phase method carbon-coated LFP material, wherein the carbon coating amount is 1wt%, the coating layer thickness is about 2nm, and the particle Dv50 is 1μm.
[0142] Comparative Example 2
[0143] The preparation method of the positive electrode material provided in this comparative example is basically the same as that in Example 1, except that in step (2), no LFO nanocrystal particles are added. That is, the positive electrode material prepared in this comparative example does not contain lithium-rich lithium ferrite.
[0144] Comparative Example 3
[0145] The preparation method of the positive electrode material provided in this comparative example is basically the same as that in Example 1, except that no LFO nanocrystalline particles are added during the hydrothermal reaction in step (2), but the obtained lithium iron phosphate material is uniformly mixed with the LFO nanocrystalline particles obtained in step (1) after sintering (ratio copper Example 1). That is, the lithium iron-rich lithium ferrate and the lithium iron phosphate material in the positive electrode material prepared in this comparative example are dispersed with each other, rather than a core-shell structure.
[0146] Comparative Example 4
[0147] The preparation method of the positive electrode material provided in this comparative example is basically the same as that in Example 1, except that, in step (2), the mass ratio of the theoretical yield (mass) of the lithium iron phosphate material to the mass ratio of the LFO nanocrystal particles is controlled to be 89:10. That is, the mass ratio of the core to the shell of the composite material with a core-shell structure in the positive electrode material prepared in this example is 0.11:1.
[0148] Experimental example
[0149] The positive electrode materials prepared in each embodiment and each comparative example were used as positive electrode active materials, and positive electrode sheets were prepared according to the following method, and then assembled into 4Ah soft-pack batteries: the positive electrode active material, SP, CNT, and PVDF were mixed and homogenized at a mass percentage of 96.5%: 1%: 0.5%: 2%, and the obtained positive electrode slurry was coated on a carbon-coated aluminum foil with a surface density of 20 mg / cm 2 , the compaction density after roller pressing is 2.6g / cm 3 The negative electrode active material is artificial graphite, and its charge capacity is 380 mAh / g. Artificial graphite, SP, CMC, and SBR are mixed uniformly at a mass percentage of 96%: 1%: 1.3%: 1.7% to obtain a negative electrode slurry, which is then coated on a 6 μm thick copper foil with a surface density of 9.75 mg / cm 2 , charging N / P is 1.06, and the compaction density after roller pressing is 1.5g / cm 3 ; After assembly, the diaphragm uses Enjie's 9+1+1 diaphragm; the composition of the electrolyte is by mass percentage: LiFP613%, EC 30%, EMC 23.5%, DMC 30%, VC 3% and DTD 0.5%. The prepared soft-pack battery was charged and discharged and the cycle performance was tested after formation. The formation voltage range was 2.0-4.2V, and the performance test voltage range was 2.0-3.65V. The 0.33C discharge gram capacity (25°C) and 0.5P / 0.5P cycle 2000 cycle capacity retention rate (25°C) of each battery are shown in Table 1 below. The viscosity change of each group of positive electrode slurry after standing for 12 hours was tested, and the results are shown in Table 1.
[0150] Table 1 Viscosity changes of each positive electrode slurry after standing for 12 hours, gram capacity of each battery and cycle capacity retention rate
[0151]
[0152]
[0153] It can be seen from Table 1 that the positive electrode slurry prepared from the positive electrode material of each embodiment has good fluidity after standing for 12 hours, and rebounds slower than that of each comparative example. It can be seen that the core-shell structure composite positive electrode material provided by the present invention has good processing performance.
[0154] Moreover, the discharge capacity of the soft pack made of the positive electrode material of each embodiment is higher than that of each comparative example. It can be seen that the core component in the composite positive electrode material has the effect of replenishing lithium and significantly improves the capacity of the positive electrode material.
[0155] In addition, the capacity retention rate of the soft pack made of the positive electrode material of each embodiment at 25°C and 1C / 1C cycle for 2000 cycles is higher than that of each comparative example. Among them, the capacity retention rate of the soft pack made of the positive electrode material of Example 1 at 25°C and 1C / 1C cycle for 2000 cycles is 99.2% (as shown in Figure 1). Figure 2 As shown), while the capacity retention rate of the soft pack of comparative example 1 at 25°C and 1C / 1C cycle for 2000 cycles is 89.9% (as shown Figure 2 As shown), it can be seen that compared with the traditional solid-phase carbon-coated LFP material in Comparative Example 1, the cycle performance of the core-shell structured composite positive electrode material has been significantly improved. This is because the excess Li released by the LFO core in the composite material cannot be embedded back into the positive electrode and is stored between the graphite layers of the negative electrode, compensating for the loss of active lithium during the cycle, thereby significantly improving the cycle performance.
[0156] In summary, the positive electrode material provided by the present invention is easy to process and can effectively improve the gram capacity and cycle performance of the battery.
[0157] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.
Claims
1. A positive electrode material, characterized in that: A composite material having a core-shell structure, wherein the core of the core-shell structure comprises lithium-rich lithium ferrite, and the shell of the core-shell structure comprises lithium iron phosphate material; At least part of the surface of the composite material is partially or completely covered with a carbon coating layer.
2. The positive electrode material according to claim 1, characterized in that: At least one of the following conditions is met: (1) The mass ratio of the core to the shell of the core-shell structure is 0.01 to 0.08:1; (2) The thickness of the carbon coating layer is 1 to 10 nm; (3) The mass ratio of the carbon coating layer to the composite material is 0.5-3:97-99.5; (4) The chemical formula of the lithium iron phosphate material is LiFe 1-x M x PO4, wherein 0≤x<0.01, and M includes at least one of Ti, Zr, V, La and Sr elements.
3. The method for preparing the positive electrode material according to claim 1 or 2, characterized in that: The steps include: (a), mixing lithium-rich lithium ferrite with a lithium source, an iron source, a phosphorus source and water and subjecting the mixture to a hydrothermal reaction, and subjecting the mixture to solid-liquid separation after the hydrothermal reaction is completed to obtain a precursor; and subjecting the precursor to sintering to obtain a composite material having a core-shell structure; (b) The composite material is made into a composite material film, and the composite material film is used as a substrate, a polymer carbon source is used as an evaporation target, and a polymer layer is grown on the substrate by electron beam evaporation, and then calcined.
4. The method for preparing the positive electrode material according to claim 3, characterized in that: In step (a), at least one of the following conditions is met: (1) During the mixing process, a dopant containing M is also added, wherein M includes at least one of Ti, Zr, V, La and Sr; (2) The temperature of the hydrothermal reaction is 200 to 300° C.; (3) The hydrothermal reaction time is 8 to 12 hours; (4) The sintering temperature is 700-800° C.; (5) The sintering holding time is 5 to 10 hours; (6) The sintering atmosphere includes an inert atmosphere; (7) The particle size Dv50 of the composite material is 1 to 3 μm; (8) The particle size Dv50 of the lithium-rich lithium iron oxide is 100 to 300 nm; (9) The preparation method of the lithium-rich lithium iron oxide comprises: mixing a lithium source, an iron source and water, and performing a hydrothermal reaction at 150 to 300° C. for 5 to 12 hours, then performing solid-liquid separation, washing and drying to obtain a solid powder, and heat treating the solid powder at 700 to 800° C. for 3 to 8 hours in an inert atmosphere to obtain the lithium-rich lithium iron oxide.
5. The method for preparing the positive electrode material according to claim 3, characterized in that: In step (b), the method for preparing the composite material film comprises: mixing the composite material with a solvent to obtain a slurry; coating the slurry on a substrate, and drying to obtain a composite material film.
6. The method for preparing the positive electrode material according to claim 5, characterized in that: At least one of the following conditions is met: (1) The solvent includes at least one of NMP, anhydrous ethanol and isopropanol; (2) after the composite material and the solvent are mixed, ball milling is performed; (3) The solid content of the slurry is 40% to 50%; (4) The coating method includes spin coating; the spin coating method includes: dropping the slurry on the substrate, letting it stand for 3 to 10 minutes, centrifuging at a speed of 1800 to 2300 r / min for 5 to 15 seconds, and performing the spin coating; the number of spin coating is 1 to 3 times; (5) coating until the thickness of the obtained film is 5 to 10 μm, and then drying; (6) The drying temperature is 80-100° C. and the drying time is 2-5 hours.
7. The method for preparing the positive electrode material according to claim 3, characterized in that: In step (b), at least one of the following conditions is met: (1) The polymer carbon source comprises at least one of glucose, polyvinyl alcohol and polyethylene glycol; (2) The thickness of the polymer layer is 1 to 5 nm; (3) The calcination temperature is 300 to 500° C. (4) The calcination time is 3 to 8 hours; (5) The calcination atmosphere includes an inert atmosphere.
8. The method for preparing the positive electrode material according to claim 3, characterized in that: After step (b), the method further includes the following steps: (c) crushing the carbon-containing composite layer obtained after calcination in step (b), then making it into a film and growing a polymer layer on its surface, and then calcining it; repeating step (c) at least 3 times; wherein the material is crushed to a particle size Dv50 of 0.5 to 2 μm.
9. A positive electrode sheet, characterized in that: The invention comprises the positive electrode material as claimed in any one of claims 1 to 2, or the positive electrode material prepared by the method for preparing the positive electrode material according to any one of claims 3 to 8.