Platinum-copper alloy catalyst for improving durability of particles and preparation method and application of platinum-copper alloy catalyst

By preparing platinum-copper alloy catalysts with nanoparticles of specific morphology and size, the problem of insufficient durability of platinum-copper alloy catalysts in the prior art has been solved, and efficient oxygen reduction and improved stability of fuel cells have been achieved.

CN119050391APending Publication Date: 2024-11-29WUXI WEIFU HIGH TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411164397.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing platinum-copper alloy catalysts have insufficient particle durability in the oxygen reduction reaction, resulting in a shortened fuel cell lifespan.

Method used

A one-step method was used to prepare platinum-copper alloy catalysts. By controlling the molar ratio of platinum salt and copper salt, the use of complexing agents, and the co-reduction reaction, nanoparticles with specific morphology and size were formed, which enhanced the antioxidant capacity of copper and optimized the nanostructure of the catalyst.

Benefits of technology

It significantly improves the particle durability of the catalyst, reduces platinum oxidation and corrosion, enhances resistance to impurities, maintains catalytic activity and stability, reduces platinum usage and agglomeration risk, and extends the service life of fuel cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050391A_ABST
    Figure CN119050391A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of catalysts, and particularly relates to a platinum-copper alloy catalyst for improving particle durability and a preparation method and application thereof. Comprising the following steps: (1) dissolving platinum salt and copper salt in deionized water, adding carbon powder, controlling the solid content of slurry to be 0.5-3%, then adding a complexing agent, and dispersing to form uniform slurry; (2) the slurry is heated to 100-170 DEG C, the slurry and a reducing agent solution enter a Y-shaped reactor at the same time for a continuous flow reaction and a co-reduction reaction, the temperature is kept at 100-170 DEG C in a heating reflux pipe, the reaction retention time is 1-24 h, and the slurry is collected into a constant-temperature kettle and cured at 25-50 DEG C for 24-240 h; and (3) carrying out solid-liquid separation on the cured slurry, carrying out vacuum drying on the precipitate obtained by washing, introducing nitrogen, and continuously drying to obtain the platinum-copper alloy catalyst. According to the platinum-copper alloy catalyst, the durability of catalyst particles in an oxygen reduction reaction can be remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of catalysts, and in particular relates to a platinum-copper alloy catalyst for improving particle durability, and a preparation method and application thereof. Background Art

[0002] Oxygen reduction reaction (ORR) plays an extremely important role in fuel cells. Its efficiency and performance directly affect the overall performance and life of the fuel cell. The stability of the oxygen reduction reaction is crucial to the life of the fuel cell. Side reactions that occur during the reaction (such as excessive reduction of oxygen) can cause corrosion and performance degradation of electrode materials, thereby shortening the battery life. Therefore, improving the durability of oxygen reduction reaction catalyst particles is crucial to the application of fuel cells.

[0003] Currently, the most commonly used oxygen reduction catalyst is platinum, but the high cost and high potential corrosion resistance of platinum have prompted researchers to look for cheaper and more reliable catalysts. Platinum-copper alloy catalysts have gradually become a research hotspot due to their excellent stability. Current research focuses on improving the performance and reliability of catalysts by regulating the structure of catalysts, including precise control of the morphology, size and composition of platinum-copper alloy catalysts to optimize their electrochemical active area and stability.

[0004] In terms of improving the durability of catalyst particles, researchers have explored a variety of methods, such as improving the dispersibility of the catalyst, enhancing the interaction between it and the carrier, and developing more stable catalysts. However, there is no method for preparing a platinum-copper alloy catalyst that can effectively improve the durability of particles. The present invention provides a method for efficiently synthesizing a platinum-copper alloy catalyst, and the synthesized catalyst has excellent particle durability. Summary of the invention

[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a platinum-copper alloy catalyst with improved particle durability and a preparation method and application thereof. The platinum-carbon alloy catalyst prepared by the preparation method of the present invention can significantly improve the durability of catalyst particles in oxygen reduction reaction, thereby solving the problem of insufficient durability of platinum-copper alloy catalyst particles in the prior art.

[0006] In order to achieve the above technical objectives, the technical solution adopted by the embodiment of the present invention is: In a first aspect, an embodiment of the present invention provides a method for preparing a platinum-copper alloy catalyst for improving particle durability, comprising the following steps: (1) Preparing a reaction slurry: dissolving platinum salt and copper salt in deionized water, stirring until completely dissolved, adding carbon powder to the solution, controlling the solid content of the slurry to be 0.5-3%, then adding a complexing agent, and dispersing for 0.5-40 hours to form a uniform slurry; (2) Slurry one-step reaction: The slurry obtained in step (1) is heated to 100-170°C, and simultaneously introduced into a Y-type reactor with a reducing agent solution for continuous flow reaction, and a co-reduction reaction is performed. The temperature in the heating reflux tube is maintained at 100-170°C, and the reaction residence time is 1-24 hours. After the reaction, the slurry is collected in a thermostatic kettle and aged at 25-50°C for 24-240 hours; (3) Washing and drying: The solution matured in step (2) is subjected to solid-liquid separation, and the precipitate is collected and washed with deionized water to remove impurities. The washed precipitate is vacuum dried at 60-80° C. for 4-24 h, and nitrogen is introduced and further dried for 0.5-8 h to obtain a highly durable platinum-copper alloy catalyst.

[0007] Furthermore, the platinum salt in step (1) is one or more of chloroplatinic acid hexahydrate, potassium chloroplatinate, platinum nitrate, platinum acetate, platinum dichloride and dinitrosodiamine platinum; The copper salt is one or more of copper chloride, copper sulfate, copper nitrate, copper acetate and copper carbonate; The molar ratio of platinum in the platinum salt to copper in the copper salt is 0.75-4.

[0008] Furthermore, the complexing agent in step (1) is one or more of triphenylphosphine, 1,3-propylene glycol, triethylamine, ethylene glycol, ethylenediaminetetraacetic acid, 2-diphenylphosphineethylamine, propanol, triphenyl phosphite, acetic acid and 1,2-diaminoethanol; The mass ratio of the complexing agent to the slurry is 0.01-0.6.

[0009] Furthermore, the ratio of the mass of the carbon powder in step (1) to the mass of the platinum element in the platinum salt and the mass of the copper element in the copper salt is 1-1.2.

[0010] Furthermore, the reducing agent solution in step (2) is a solution of one or more of sodium sulfate, hydrazine hydrate, sodium borohydride, sodium dithionite, sodium sulfite and diisobutylaluminum hydride; The reducing agent solution has the same temperature and volume as the slurry, and the mass concentration of the reducing agent solution is 2-15%.

[0011] Furthermore, the reaction convergence angle of the Y-type reactor in step (2) is 60-120°.

[0012] Furthermore, in step (2), the temperature in the heating reflux tube is maintained at 120-160°C; After the reaction in step (2), the slurry is collected in a thermostatic kettle and aged at 25-40° C. for 24-240 hours.

[0013] In a second aspect, an embodiment of the present invention provides a platinum-copper alloy catalyst prepared by the preparation method described in the first aspect.

[0014] In a third aspect, an embodiment of the present invention provides an application of the platinum-copper alloy catalyst described in the second aspect in a proton exchange membrane fuel cell.

[0015] The technical solution provided by the embodiment of the present invention has the following beneficial effects: 1. The copper element in the platinum-copper alloy catalyst can enhance the antioxidant capacity of platinum, reduce the oxidation and corrosion of platinum during the operation of the fuel cell, and thus improve the overall stability of the catalyst.

[0016] 2. The platinum-copper alloy catalyst prepared by the present invention can optimize its nanostructure by regulating the alloy composition and preparation method to form nanoparticles with specific morphology and size. These structures can better resist structural degradation during long-term operation.

[0017] 3. Platinum-copper alloy catalysts have better resistance to impurities (such as sulfur, nitrogen compounds, etc.) that may be encountered during fuel cell operation, which helps maintain the activity and stability of the catalyst.

[0018] 4. Pt-Cu alloy catalysts can improve the kinetics of oxygen reduction reaction (ORR), allowing efficient oxygen reduction at lower overpotentials, which helps reduce catalyst degradation caused by high overpotentials.

[0019] 5. By alloying with copper, the amount of platinum can be reduced while maintaining a high catalytic activity, which not only reduces costs, but also reduces the risk of agglomeration and dissolution of platinum due to the reduction in the total amount of platinum, thereby improving the durability of the catalyst.

[0020] 6. At the same platinum loading, the alloy catalyst can provide more catalytic active sites, which helps to improve the performance and service life of the catalyst.

[0021] 7. The preparation method of the platinum-copper alloy catalyst of the present invention is simple, and the platinum-copper alloy catalyst is prepared in one step, which is easy to operate and reduces the loss of precious metals in the preparation process, which is conducive to industrial production.

[0022] 8. The present invention improves the activity and stability of the catalyst and prolongs the service life of the fuel cell by optimizing the preparation process. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a schematic diagram of the preparation process of the fuel cell platinum-copper alloy catalyst for improving particle durability of the present invention.

[0024] Figure 2It is the X-ray powder diffraction pattern of the platinum-copper alloy catalyst prepared in Example 1 and Example 3 of the present invention.

[0025] Figure 3 It is a comparison diagram of linear voltammetric scanning curves of particle durability test before and after 30,000 square wave cycles in a three-electrode system of a platinum-copper alloy catalyst prepared in Example 2 of the present invention.

[0026] Figure 4 It is a comparison diagram of linear voltammetric scanning curves of particle durability test before and after 30,000 square wave cycles in a three-electrode system of a platinum-copper alloy catalyst prepared in Comparative Example 2 of the present invention. DETAILED DESCRIPTION

[0027] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0028] Example 1 A method for preparing a platinum-copper alloy catalyst for improving particle durability comprises the following steps: (1) Dissolve 1.32 g of chloroplatinic acid hexahydrate and 0.11 g of cupric chloride dihydrate in deionized water and stir until completely dissolved. Add 0.54 g of carbon powder to the solution, and the solid content of the slurry is 0.5%. Then add 5.4 g of 1,2-diaminoethanol and 59.4 g of propanol and fully disperse for 0.5 h to form a uniform slurry. (2) The slurry is heated to 170°C and introduced into a Y-type reactor with a reaction confluence angle of 60° to carry out a continuous flow reaction with an aqueous solution of sodium dithionite having the same temperature, volume and mass concentration of 2%, and to carry out a co-reduction reaction, such as Figure 1 As shown, the temperature in the heating reflux tube was maintained at 170°C, the reaction residence time was 1h, and the slurry after the reaction was collected in a thermostatic kettle and aged at 25°C for 240h; (3) The solution matured in step (2) is subjected to solid-liquid separation, and the precipitate is collected and washed with deionized water to remove impurities. The washed precipitate is vacuum dried at 80° C. for 24 h, and nitrogen is introduced and further dried for 0.5 h to obtain a highly durable platinum-copper alloy catalyst.

[0029] Example 2 A method for preparing a platinum-copper alloy catalyst for improving particle durability, which differs from Example 1 in that the platinum salt used in step (1) is platinum nitrate, the copper salt is copper nitrate, the reducing agent used in step (2) is hydrazine hydrate, and other conditions and proportions are the same as those in Example 1.

[0030] Example 3 A method for preparing a platinum-copper alloy catalyst for improving particle durability, which differs from Example 1 in that the complexing agent used in step (1) is 5.8 g of 2-diphenylphosphineethylamine and 61.3 g of ethylene glycol, and other conditions and proportions are the same as those in Example 1.

[0031] Example 4 A method for preparing a platinum-copper alloy catalyst for improving particle durability, which differs from Example 3 in that in step (2), the temperature in the heating reflux tube is maintained at 120° C. and the reaction residence time is 24 h. After the reaction, the slurry is collected in a constant temperature kettle and aged at 50° C. for 24 h. Other conditions and proportions are the same as those in Example 3.

[0032] Comparative Example 1 A method for preparing a platinum-copper alloy catalyst for improving particle durability comprises the following steps: (1) Dissolve 1.32 g of chloroplatinic acid hexahydrate and 0.11 g of cupric chloride dihydrate in deionized water and stir until completely dissolved. Add 0.54 g of carbon powder to the solution, and add 5.4 g of 1,2-diaminoethanol and 59.4 g of propanol to form a uniform slurry. Disperse for 0.5 h. (2) The reaction slurry is heated to 170° C. and introduced into a Y-type reactor with a reaction confluence angle of 60° to carry out a continuous flow reaction with an aqueous solution of sodium dithionite of the same temperature, volume and mass concentration of 2% to carry out a co-reduction reaction. The temperature in the heating reflux tube is maintained at 170° C. The reaction residence time is 1 hour. The slurry after the reaction is not subjected to an aging step; (3) The reaction liquid in step (2) is subjected to solid-liquid separation, and the precipitate is collected and washed with deionized water to remove impurities. The washed precipitate is vacuum dried at 80° C. for 24 h, and nitrogen is introduced and further dried for 0.5 h to obtain a highly durable platinum-copper alloy catalyst.

[0033] Comparative Example 2 A method for preparing a platinum-copper alloy catalyst for improving particle durability, which differs from Example 2 in that 5.4 g of 1,2-diaminoethanol and 59.4 g of propanol (complexing agent) are not added in step (1), and other conditions and proportions are the same as those in Example 2.

[0034] from Figure 2 It can be seen that the characteristic diffraction peaks of platinum (111), (200), and (220) are all shifted to the right, indicating that a platinum-copper alloy catalyst structure is prepared after a one-step slurry reaction.

[0035] Figure 3 It is a comparison diagram of linear voltammetric scanning curves of the particle durability test after 30,000 square wave cycles of the platinum-copper alloy catalyst prepared in Example 2 of the present invention under the three-electrode system. Figure 4It is a comparison diagram of linear voltammetric scanning curves of particle durability test after 30,000 square wave cycles of the platinum-copper alloy catalyst prepared in comparative example 2 of the present invention under a three-electrode system.

[0036] Figure 3 and 4 Electrochemical performance test conditions: three-electrode system, electrolyte is oxygen-saturated 0.1M HClO4; rotation speed: 1600rpm; scan rate: 10 mVs -1 ; The 30,000 endurance attenuation condition is to conduct a square wave test, at 0.6V and 0.95 Vvs.RHE, the two test voltages stay for 3s, and a test cycle is completed in 6s, scanning 10,000, 20,000, and 30,000 circles, the test scan rate is 20 mV / s for CV and LSV, and the mass activity is calculated until 30,000 circles, and the constant temperature water bath is 25°C.

[0037] from Figure 3 It can be seen that the initial mass activity is 0.307 A / mg. After 30,000 cycles of endurance cycling, the mass activity of the catalyst decays slightly, with a decay rate of only 8.1%.

[0038] As can be seen from Figure 4, the initial mass activity of the catalyst prepared in Comparative Example 2 is 0.213 A / mg. After 30,000 cycles of endurance cycling in the three-electrode system, the mass activity of the catalyst decays significantly, with a decay rate of 48.8%.

[0039] and Figure 3 Compared with the results of Example 2, the initial mass activity of Example 2 is 30.6% higher than that of Comparative Example 2; by comparing Example 2 with Comparative Example 2, it can be found that the durability attenuation decreases from 48.8% to 8.1%, and the attenuation rate decreases significantly, which indicates that the particle durability of the catalyst prepared by the preparation method of the present invention is significantly improved.

[0040] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.

Claims

1. A method for preparing a platinum-copper alloy catalyst for improving particle durability, characterized in that: The following steps are involved: (1) Preparing a reaction slurry: dissolving platinum salt and copper salt in deionized water, stirring until completely dissolved, adding carbon powder to the solution, controlling the solid content of the slurry to be 0.5-3%, then adding a complexing agent, and dispersing for 0.5-40 hours to form a uniform slurry; (2) Slurry one-step reaction: The slurry obtained in step (1) is heated to 100-170°C, and simultaneously introduced into a Y-type reactor with a reducing agent solution for continuous flow reaction, and a co-reduction reaction is performed. The temperature in the heating reflux tube is maintained at 100-170°C, and the reaction residence time is 1-24 hours. After the reaction, the slurry is collected in a thermostatic kettle and aged at 25-50°C for 24-240 hours; (3) Washing and drying: The solution matured in step (2) is subjected to solid-liquid separation, and the precipitate is collected and washed with deionized water to remove impurities. The washed precipitate is vacuum dried at 60-80° C. for 4-24 h, and nitrogen is introduced and further dried for 0.5-8 h to obtain a highly durable platinum-copper alloy catalyst.

2. The method for preparing a platinum-copper alloy catalyst for improving particle durability according to claim 1, characterized in that: The platinum salt in step (1) is one or more of chloroplatinic acid hexahydrate, potassium chloroplatinate, platinum nitrate, platinum acetate, platinum dichloride and dinitrosodiamine platinum; The copper salt is one or more of copper chloride, copper sulfate, copper nitrate, copper acetate and copper carbonate; The molar ratio of platinum in the platinum salt to copper in the copper salt is 0.75-4.

3. The method for preparing a platinum-copper alloy catalyst for improving particle durability according to claim 1, characterized in that: The complexing agent in step (1) is one or more of triphenylphosphine, 1,3-propylene glycol, triethylamine, ethylene glycol, ethylenediaminetetraacetic acid, 2-diphenylphosphineethylamine, propanol, triphenyl phosphite, acetic acid and 1,2-diaminoethanol; The mass ratio of the complexing agent to the slurry is 0.01-0.

6.

4. The method for preparing a platinum-copper alloy catalyst for improving particle durability according to claim 1, characterized in that: The ratio of the mass of the carbon powder in step (1) to the mass of the platinum element in the platinum salt and the mass of the copper element in the copper salt is 1-1.

2.

5. The method for preparing a platinum-copper alloy catalyst for improving particle durability according to claim 1, characterized in that: The reducing agent solution in step (2) is a solution of one or more of sodium sulfate, hydrazine hydrate, sodium borohydride, sodium dithionite, sodium sulfite and diisobutylaluminum hydride; The reducing agent solution has the same temperature and volume as the slurry, and the mass concentration of the reducing agent solution is 2-15%.

6. The method for preparing a platinum-copper alloy catalyst for improving particle durability according to claim 1, characterized in that: The reaction convergence angle of the Y-type reactor in step (2) is 60-120°.

7. The method for preparing a platinum-copper alloy catalyst for improving particle durability according to claim 1, characterized in that: In step (2), the temperature in the heating reflux tube is maintained at 120-160°C; After the reaction in step (2), the slurry is collected in a thermostatic kettle and aged at 25-40° C. for 24-240 hours.

8. A platinum-copper alloy catalyst, characterized in that: The method is prepared by the preparation method according to any one of claims 1 to 7.

9. Use of the platinum-copper alloy catalyst according to claim 8 in a proton exchange membrane fuel cell.