Cross-linked proton exchange membrane and preparation method thereof
By forming a polyion liquid crosslinking structure in the perfluorosulfonic acid proton exchange membrane, the problems of its reduced proton conductivity and poor mechanical properties under low humidity conditions are solved, and the stability and service life of the membrane are improved.
Patent Information
- Application Number
- CN202410994532.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-29
AI Technical Summary
The perfluorosulfonic acid proton exchange membrane has a reduced proton conductivity and poor mechanical properties under low humidity conditions, which affects its long-term durability.
The design of crosslinked proton exchange membrane, including polymer matrix, silane coupling agent, initiator and functional regulator, forms a polyion liquid crosslinking structure through grafting and crosslinking reactions, enhancing the density and mechanical properties of the membrane. .
It improves the working stability and mechanical properties of the crosslinked proton exchange membrane under low humidity conditions, extends its service life, and prevents ionic liquid from leaching under low humidity conditions.
Smart Images

Figure CN119050428A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of proton exchange membranes, and in particular to a cross-linked proton exchange membrane and a preparation method thereof. Background Art
[0002] Currently, the most widely used proton exchange membrane is the perfluorosulfonic acid proton exchange membrane, but this type of proton exchange membrane is highly dependent on humidity. The ion channels of the perfluorosulfonic acid proton exchange membrane are prone to collapse in a dry state, which limits the proton conduction process of the perfluorosulfonic acid proton exchange membrane. In addition, with the continuous development of fuel cells, proton exchange membranes are inevitably used in various harsh environments such as low humidity and high temperature. Therefore, providing more effective, stable, lightweight and low-cost proton exchange membranes to cope with harsh environments such as low humidity and high temperature is the current direction pursued by the development of proton exchange membranes. At present, based on the high proton conductivity and water-independence of ionic liquids (ILs), as well as the excellent properties of Ils such as high ionic conductivity, high thermal stability and strong chemical stability, the use of ILs as a proton conduction carrier to modify the perfluorosulfonic acid proton exchange membrane can significantly improve the proton conductivity of the perfluorosulfonic acid proton exchange membrane under low humidity conditions. Therefore, Ils is generally used as the electrolyte of the perfluorosulfonic acid proton exchange membrane. In addition, current studies have shown that if the perfluorosulfonic acid proton exchange membrane has a higher sulfonate concentration, the decrease in its proton conductivity under low humidity conditions is smaller; in addition, studies have shown that optimizing the side chain structure of perfluorosulfonic acid can promote the separation of the hydrophobic-hydrophilic domains of the perfluorosulfonic acid proton exchange membrane, which is beneficial to the construction of an efficient proton transport channel in the perfluorosulfonic acid proton exchange membrane; therefore, increasing the sulfonate concentration and optimizing the side chain structure of perfluorosulfonic acid under the premise of adding Ils to the fluorosulfonic acid proton exchange membrane are effective ways to improve the proton conductivity of the perfluorosulfonic acid proton exchange membrane under low relative humidity (RH) conditions.
[0003] However, due to the plasticizing effect of ILs, the mechanical properties of the perfluorosulfonic acid proton exchange membrane will decrease significantly with the increase of the ILs content doped in the perfluorosulfonic acid proton exchange membrane. In addition, during the operation of the fuel cell, excessive Ils will also leach out of the perfluorosulfonic acid proton exchange membrane, which will affect the long-term durability of the perfluorosulfonic acid proton exchange membrane. Summary of the invention
[0004] The present application provides a cross-linked proton exchange membrane and a preparation method thereof to solve the following technical problem: how to improve the long-term durability of a perfluorosulfonic acid proton exchange membrane.
[0005] In a first aspect, the present application provides a cross-linked proton exchange membrane, wherein the raw materials of the cross-linked proton exchange membrane include: a polymer matrix, a silane coupling agent, an initiator and a functional regulator, wherein the mass ratio of the silane coupling agent to the polymer matrix is ≥0.03:1, the mass ratio of the initiator to the polymer matrix is ≥0.01:1, and the mass ratio of the functional regulator to the polymer matrix is ≥1:1;
[0006] Wherein, the raw materials of the polymer matrix include amino monomers and perfluorosulfonic acid resin, and the molar ratio of the amino monomers to the perfluorosulfonic acid resin is ≥2:1;
[0007] The functional regulator includes sulfonate and / or phosphoric acid.
[0008] Optionally, the molar ratio of the amino monomer to the perfluorosulfonic acid resin is (2:1) to (5:1).
[0009] Optionally, the amino monomer includes N,N-dimethylethylenediamine monomer.
[0010] Optionally, the polymer matrix has a molecular structure as shown in Formula 1,
[0011]
[0012] In formula 1, x≥2.
[0013] Optionally, the functional regulator includes trifluoromethanesulfonic acid.
[0014] Optionally, when the functional regulator is trifluoromethanesulfonic acid, the cross-linked proton exchange membrane has a molecular structure as shown in Formula 2,
[0015]
[0016] In formula 2, x≥2.
[0017] Optionally, when the functional regulator is phosphoric acid, the cross-linked proton exchange membrane has a molecular structure as shown in Formula 3,
[0018]
[0019] In formula 3, x≥2.
[0020] In a second aspect, the present application provides a method for preparing the cross-linked proton exchange membrane according to the first aspect, the method comprising:
[0021] A dispersion of a perfluorosulfonic acid resin solution and an amino monomer are subjected to a graft reaction to obtain a first reaction solution;
[0022] The first reaction liquid is dried and then calcined to obtain a polymer matrix;
[0023] Performing a cross-linking reaction on the initiator, the silane coupling agent and the polymer matrix to obtain a second reaction solution;
[0024] The second reaction liquid is dried, and then annealed and membrane stripped to obtain a coarse-grade cross-linked proton exchange membrane;
[0025] The coarse-grade cross-linked proton exchange membrane is immersed in a functional regulator, and then purified to obtain a cross-linked proton exchange membrane.
[0026] Optionally, the temperature of the grafting reaction is 20° C. to 30° C., and the time of the grafting reaction is 12 h to 24 h.
[0027] Optionally, the calcination temperature is 215° C. to 235° C., and the calcination time is 1 h to 2 h.
[0028] Optionally, the temperature of the cross-linking reaction is 135° C. to 145° C., and the time of the cross-linking reaction is ≥ 12 h.
[0029] Optionally, the annealing temperature is 115° C. to 125° C., and the annealing time is ≥ 2 h.
[0030] Optionally, the immersion temperature is 75° C. to 85° C., and the immersion time is ≥ 12 h.
[0031] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:
[0032] An embodiment of the present application provides a cross-linked proton exchange membrane, wherein the raw materials of the cross-linked proton exchange membrane include: a polymer matrix, a silane coupling agent, an initiator and a functional regulator, wherein the mass ratio of the silane coupling agent to the polymer matrix is ≥0.03:1, the mass ratio of the initiator to the polymer matrix is ≥0.01:1, and the mass ratio of the functional regulator to the polymer matrix is ≥1:1; wherein the raw materials of the polymer matrix include an amino monomer and a perfluorosulfonic acid resin, and the molar ratio of the amino monomer to the perfluorosulfonic acid resin is ≥2:1; and the functional regulator includes a sulfonate and / or phosphoric acid. The raw materials of the polymer matrix may include an amino monomer and a perfluorosulfonic acid resin, and the molar ratio of the amino monomer to the perfluorosulfonic acid resin is generally ≥2, which can promote the sulfonic acid group of the perfluorosulfonic acid resin to fully react with the amino group of the amino monomer to promote the amino group to be grafted onto the side chain of the perfluorosulfonic acid resin. In addition, the mass ratio of the initiator to the polymer matrix is generally ≥0.01:1, which can promote the side chain of the perfluorosulfonic acid resin grafted with the amino group to be fully connected with the silane coupling agent under the initiation of the initiator. In addition, the mass ratio of the silane coupling agent to the polymer matrix is generally ≥0.03:1, which can promote the perfluorosulfonic acid resin connected with the silane coupling agent to fully undergo in-situ free radical polymerization to form a sufficient cross-linking structure. In addition, the mass ratio of the functional regulator to the polymer matrix is ≥1:1, and the functional regulator may include sulfonic acid Salt and / or phosphoric acid, so that a sufficient amount of cross-linking structure is connected to the functional regulator through ionic bonds, and a sufficient amount of polyionic liquid cross-linking structure can be formed. On the one hand, a sufficient amount of polyionic liquid cross-linking structure can prevent the ionic liquid from leaching from the system under low relative humidity conditions, so as to enhance the compactness of the cross-linked proton exchange membrane while maintaining the mechanical properties of the cross-linked proton exchange membrane, thereby improving the working stability of the cross-linked proton exchange membrane under low relative humidity conditions, so as to improve the durability of the perfluorosulfonic acid proton exchange membrane. On the other hand, a sufficient amount of polyionic liquid cross-linking structure can promote the close adhesion of the cross-linked proton exchange membrane to the catalyst layer and the frame material of the sealing ring, so as to effectively prevent the peeling of the cross-linked proton exchange membrane and the catalyst layer, and delay the aging of the frame material of the sealing ring, thereby improving the service life of the perfluorosulfonic acid proton exchange membrane. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0034] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0035] Figure 1 A schematic diagram of the synthesis principle of a cross-linked proton exchange membrane provided in an embodiment of the present application;
[0036] Figure 2 A schematic diagram of the synthesis principle of a polymer matrix in a cross-linked proton exchange membrane provided in an embodiment of the present application;
[0037] Figure 3 A schematic flow chart of a method for preparing a cross-linked proton exchange membrane provided in an embodiment of the present application. DETAILED DESCRIPTION
[0038] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0039] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity and should not be understood as a rigid limitation on the scope of the present application; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values within the range; for example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which applies regardless of the range; in addition, whenever a numerical range is indicated in this document, it is meant to include any cited numbers (fractions or integers) within the indicated range.
[0040] In this document, the terms including "comprising" and the like mean "including but not limited to". Relational terms such as "first" and "second" are merely used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. "And / or" describes the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone; wherein A and B can be singular or plural. Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased on the market or prepared by existing methods.
[0041] It should be noted that the molecular formula of silane coupling agent can generally be expressed as R nIt is represented by the general formula SiX, where n<4 and n is a natural number. The characteristic of silane coupling agent is that it has two or more different reactive groups in the molecule. The R group is a non-hydrolyzable group that can react with organic matter, such as vinyl, allyl, hydrogen, epoxy, mercapto, acryloxypropyl, etc. The X group is an indispensable group for reacting with inorganic materials and is also a hydrolyzable group, such as methoxy, ethoxy, acyloxy, aryloxy, tert-butyl peroxy, chlorine, etc. The silane coupling agent generates Si-OH group after hydrolysis, and the generated Si-OH group can condense with inorganic materials such as carbon black. Among them, the structure of silane coupling agent KH560 is shown in formula 4,
[0042]
[0043] However, in the coupling mechanism of silane coupling agent KH560, silane coupling agent contains epoxy groups, which enable silane coupling agent KH560 to form hydrogen bonds or covalent bonds with functional groups, thereby enabling silane coupling agent to crosslink polymer macromolecule structure, and in the process of crosslinking and curing, silane coupling agent and polymer macromolecule will form a dense three-dimensional network structure, thereby improving the density of the material and enhancing the various properties of the material. In addition, silane coupling agent has low surface energy and high wetting ability, and can be evenly distributed in the resin solution, so silane coupling agent can also be used as a sealant. This type of sealant can be added to the polymer resin solution to form a proton exchange membrane through solution casting. In the subsequent fuel cell work, this type of sealant can also improve the adhesion between the proton exchange membrane and the catalyst layer and the sealing ring, thereby effectively preventing the peeling of the catalyst layer and the proton membrane, and can also delay the aging of the sealing ring frame material, thereby improving the durability of the fuel cell.
[0044] Figure 1 The schematic diagram of the synthesis principle of a cross-linked proton exchange membrane provided in an embodiment of the present application is exemplarily shown;
[0045] like Figure 1 As shown, an embodiment of the present application provides a cross-linked proton exchange membrane, wherein the raw materials of the cross-linked proton exchange membrane include: a polymer matrix, a silane coupling agent, an initiator and a functional regulator, wherein the mass ratio of the silane coupling agent as a molecule to the polymer matrix as a denominator is ≥0.03:1, the mass ratio of the initiator as a molecule to the polymer matrix as a denominator is ≥0.01:1, and the mass ratio of the functional regulator as a molecule to the polymer matrix as a denominator is ≥1:1;
[0046] The raw materials of the polymer matrix include amino monomers and perfluorosulfonic acid resin, and the molar ratio of the amino monomer as a numerator and the perfluorosulfonic acid resin as a denominator is ≥2:1;
[0047] The functional regulator includes sulfonate and / or phosphoric acid.
[0048] It should be noted that by introducing an amino monomer into the perfluorosulfonic acid resin, the perfluorosulfonic acid resin and the silane coupling agent can be connected through the amino group of the amino monomer to form a cross-linked structure of the perfluorosulfonic acid resin; in addition, the amino group of the amino monomer can also connect the perfluorosulfonic acid resin and the functional regulator through an ion bond to obtain a cross-linked proton exchange membrane with different chain lengths, which is convenient for actual use needs.
[0049] In some optional embodiments, the molar ratio of the amino monomer as a numerator and the perfluorosulfonic acid resin as a denominator is (2:1) to (5:1);
[0050] In these embodiments, the molar ratio of the amino monomer as the molecule and the perfluorosulfonic acid resin as the denominator can be (2:1) to (5:1), which can further promote the sulfonic acid group of the perfluorosulfonic acid resin to fully react with the amino group of the amino monomer to promote the amino group to be grafted onto the side chain of the perfluorosulfonic acid resin. The perfluorosulfonic acid resin grafted with the amino group can be subsequently connected with a silane coupling agent and a functional regulator, respectively, so as to obtain a sufficient amount of polyionic liquid cross-linked structure.
[0051] The molar ratio of the amine monomer as a numerator and the perfluorosulfonic acid resin as a denominator may be 2:1, 3:1, 4:1 or 5:1.
[0052] In some optional embodiments, the amine monomer includes N,N-dimethylethylenediamine monomer;
[0053] In these embodiments, the amino monomer may include N,N-dimethylethylenediamine monomer, which can promote the amino monomer to have a sufficient amount of amino group, and the sufficient amount of amino group can fully undergo a grafting reaction with the sulfonic acid group of the perfluorosulfonic acid resin to promote the amino group to be grafted onto the side chain of the perfluorosulfonic acid resin. The perfluorosulfonic acid resin grafted with the amino group can subsequently be connected with a silane coupling agent and a functional regulator, respectively, so as to obtain a sufficient amount of polyionic liquid cross-linked structure.
[0054] It should be noted that the N,N-dimethylethylenediamine monomer not only has sufficient amino groups, but also has a relatively low boiling point (105° C.), and can be removed from the polymer matrix during the subsequent thermally induced dehydration process, thereby improving the purity of the polymer matrix.
[0055] In some optional embodiments, the polymer matrix has a molecular structure as shown in Formula 1,
[0056]
[0057] In formula 1, x ≥ 2;
[0058] In these embodiments, it is clear that the polymer matrix has a molecular structure as shown in Formula 1, and the binding sites of the sulfonic acid group of the perfluorosulfonic acid resin and the amino monomer can be clearly identified, thereby facilitating the subsequent connection of the polymer matrix with the silane coupling agent and the functional regulator, respectively, so as to obtain a sufficient amount of polyionic liquid cross-linked structure.
[0059] In some optional embodiments, the functional modulator includes trifluoromethanesulfonic acid;
[0060] In these embodiments, the functional regulator may include trifluoromethanesulfonic acid, so that the polymer matrix can introduce fluorine and other groups while introducing sulfonic acid groups to extend the chain length of the polymer matrix, thereby preventing the ionic liquid from leaching from the system under low relative humidity conditions, thereby enhancing the compactness of the cross-linked proton exchange membrane while maintaining the mechanical properties of the cross-linked proton exchange membrane, thereby improving the working stability of the cross-linked proton exchange membrane under low relative humidity conditions, and improving the durability of the perfluorosulfonic acid proton exchange membrane.
[0061] In some optional embodiments, when the functional regulator is trifluoromethanesulfonic acid, the cross-linked proton exchange membrane has a molecular structure as shown in Formula 2,
[0062]
[0063] In formula 2, x ≥ 2;
[0064] In these embodiments, when the functional regulator is trifluoromethanesulfonic acid, the cross-linked proton exchange membrane can have a molecular structure as shown in Formula 2, which can clarify the binding sites of the polymer matrix with the silane coupling agent and the functional regulator, and at the same time indicate that the exchange proton membrane has a sufficient amount of polyionic liquid cross-linking structure. On the one hand, a sufficient amount of polyionic liquid cross-linking structure can prevent the ionic liquid from leaching from the system under low relative humidity conditions, so as to enhance the compactness of the cross-linked proton exchange membrane while maintaining the mechanical properties of the cross-linked proton exchange membrane, thereby improving the working stability of the cross-linked proton exchange membrane under low relative humidity conditions, so as to improve the durability of the perfluorosulfonic acid proton exchange membrane. On the other hand, a sufficient amount of polyionic liquid cross-linking structure can promote the close adhesion of the cross-linked proton exchange membrane to the catalyst layer and the frame material of the sealing ring, so as to effectively prevent the peeling of the cross-linked proton exchange membrane and the catalyst layer, and delay the aging of the frame material of the sealing ring, thereby improving the service life of the perfluorosulfonic acid proton exchange membrane.
[0065] In some optional embodiments, when the functional regulator is phosphoric acid, the cross-linked proton exchange membrane has
[0066] The molecular structure shown in formula 3,
[0067]
[0068] In formula 3, x ≥ 2;
[0069] In these embodiments, when the functional regulator is a phosphate group, the cross-linked proton exchange membrane can have a molecular structure as shown in Formula 3, which can clarify the binding sites of the polymer matrix with the silane coupling agent and the functional regulator, and at the same time indicate that the exchange proton membrane has a sufficient amount of polyionic liquid cross-linking structure. On the one hand, a sufficient amount of polyionic liquid cross-linking structure can prevent the ionic liquid from leaching from the system under low relative humidity conditions, so as to enhance the compactness of the cross-linked proton exchange membrane while maintaining the mechanical properties of the cross-linked proton exchange membrane, thereby improving the working stability of the cross-linked proton exchange membrane under low relative humidity conditions, so as to improve the durability of the perfluorosulfonic acid proton exchange membrane. On the other hand, a sufficient amount of polyionic liquid cross-linking structure can promote the close adhesion of the cross-linked proton exchange membrane to the catalyst layer and the frame material of the sealing ring, so as to effectively prevent the peeling of the cross-linked proton exchange membrane and the catalyst layer, and delay the aging of the frame material of the sealing ring, thereby improving the service life of the perfluorosulfonic acid proton exchange membrane.
[0070] Figure 2 A schematic diagram of the synthesis principle of a polymer matrix in a cross-linked proton exchange membrane provided in an embodiment of the present application is exemplarily shown;
[0071] Figure 3 A schematic flow chart of a method for preparing a cross-linked proton exchange membrane provided in an embodiment of the present application is shown exemplarily;
[0072] Based on a general inventive concept, such as Figure 2 and Figure 3 As shown, the embodiment of the present application provides a method for preparing the cross-linked proton exchange membrane, the method comprising:
[0073] S1. A dispersion of a perfluorosulfonic acid resin solution and an amino monomer are subjected to a grafting reaction to obtain a first reaction solution;
[0074] S2. The first reaction solution is dried and then calcined to obtain a polymer matrix;
[0075] S3. cross-linking the initiator, the silane coupling agent and the polymer matrix to obtain a second reaction solution;
[0076] S4. drying the second reaction solution, and then annealing and membrane stripping to obtain a coarse-grade cross-linked proton exchange membrane;
[0077] S5. Using a functional regulator, immersing the coarse-grade cross-linked proton exchange membrane in, and then purifying to obtain a cross-linked proton exchange membrane.
[0078] This method is a method for preparing the above-mentioned cross-linked proton exchange membrane. The specific composition and structure of the cross-linked proton exchange membrane can refer to the above-mentioned embodiment. Since this method adopts part or all of the technical solutions of the above-mentioned embodiment, it at least has all the beneficial effects brought by the technical solutions of the above-mentioned embodiment, which will not be repeated here one by one.
[0079] It should be noted that the drying can be carried out in a blast oven, the drying temperature of the first reaction liquid can be 80° C., the drying temperature of the second reaction liquid can be 60° C., and the drying time of the second reaction liquid can be 12 h.
[0080] It should be noted that, for the purification, the crude cross-linked proton exchange membrane can be first washed with deionized water until it becomes neutral and then dried under reduced pressure at 80° C. for 12 h.
[0081] In some optional embodiments, the temperature of the grafting reaction is 20°C to 30°C, and the time of the grafting reaction is 12h to 24h;
[0082] In these embodiments, the temperature of the grafting reaction can be 20° C. to 30° C., and the time of the grafting reaction can be 12 h to 24 h, which can promote the complete acid-base reaction between the sulfonic acid group of the perfluorosulfonic acid resin solution and the amino group of the amino monomer, so as to promote the amino group of the amino monomer to be grafted to the side chain of the perfluorosulfonic acid, thereby obtaining a sufficient amount of the first reaction solution.
[0083] The temperature of the grafting reaction can be 20°C, 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C, 29°C or 30°C.
[0084] The grafting reaction time can be 12 h, 14 h, 16 h, 18 h, 20 h, 22 h or 24 h.
[0085] In some optional embodiments, the calcination temperature is 215°C to 235°C, and the calcination time is 1h to 2h;
[0086] In these embodiments, the calcination temperature can be 215°C to 235°C, and the calcination time can be 1h to 2h, which can promote the first reaction liquid to convert the salt into the corresponding sulfonimide by heat-induced dehydration, thereby obtaining a polymer matrix; in addition, the boiling point of the amino monomer is generally lower than 200°C, and the amino monomer can be evaporated within the calcination temperature and calcination time range to promote the separation of the amino monomer from the polymer matrix, thereby obtaining a pure polymer matrix.
[0087] The calcination temperature may be 215°C, 216°C, 217°C, 218°C, 219°C, 220°C, 221°C, 222°C, 223°C, 224°C, 225°C, 226°C, 227°C, 228°C, 229°C, 230°C, 231°C, 232°C, 233°C, 234°C or 235°C.
[0088] The calcination time may be 1 h, 1.1 h, 1.2 h, 1.3 h, 1.4 h, 1.5 h, 1.6 h, 1.7 h, 1.8 h, 1.9 h or 2.0 h.
[0089] In some optional embodiments, the temperature of the cross-linking reaction is 135° C. to 145° C., and the time of the cross-linking reaction is ≥ 12 h.
[0090] In these embodiments, the temperature of the cross-linking reaction can be 135° C. to 145° C., and the time of the cross-linking reaction is generally ≥ 12 h, which can promote the initiator, the silane coupling agent and the polymer matrix to undergo a sufficient polymerization reaction, and under the initiation of the initiator, the silane coupling agent and the perfluorosulfonic acid resin are promoted to undergo a sufficient in-situ free radical polymerization reaction to form a sufficient cross-linking structure.
[0091] The temperature of the cross-linking reaction may be 135°C, 136°C, 137°C, 138°C, 139°C, 140°C, 141°C, 142°C, 143°C, 144°C or 145°C.
[0092] In some optional embodiments, the annealing temperature is 115° C. to 125° C., and the annealing time is ≥ 2 h.
[0093] In these embodiments, the annealing temperature can be 115° C. to 125° C., and the annealing time is generally ≥ 2 hours, which can improve the crystallinity of the second reaction liquid after drying, so as to facilitate the subsequent reaction between the coarse-grade cross-linked proton exchange membrane with a cross-linked structure and the functional regulator, thereby obtaining a sufficient amount of polyionic liquid cross-linked structure.
[0094] The annealing temperature may be 115°C, 116°C, 117°C, 118°C, 119°C, 120°C, 121°C, 122°C, 123°C, 124°C or 125°C.
[0095] In some optional embodiments, the immersion temperature is 75°C to 85°C, and the immersion time is ≥12h;
[0096] In these embodiments, the immersion temperature can be 75° C. to 85° C., and the immersion time is generally ≥ 12 h, which can promote the connection between the coarse-crosslinked proton exchange membrane with a cross-linked structure and the functional regulator, thereby forming a sufficient amount of polyionic liquid cross-linked structure.
[0097] The immersion temperature may be 75°C, 76°C, 77°C, 78°C, 79°C, 80°C, 81°C, 82°C, 83°C, 84°C or 85°C.
[0098] The present application is further described below in conjunction with specific examples. The experimental methods in the following examples that do not specify specific conditions are usually measured according to industry standards; if there are no corresponding industry standards, they are carried out according to common international standards, conventional conditions, or conditions recommended by the manufacturer.
[0099] Example 1
[0100] A cross-linked proton exchange membrane, the raw materials of the cross-linked proton exchange membrane include: a polymer matrix, a silane coupling agent, an initiator and a functional regulator, the mass ratio of the silane coupling agent to the polymer matrix is 0.03, the mass ratio of the initiator to the polymer matrix is 0.01, and the mass ratio of the functional regulator to the polymer matrix is 4:1; wherein the raw materials of the polymer matrix include N,N-dimethylethylenediamine monomer and perfluorosulfonic acid resin, the molar ratio of the N,N-dimethylethylenediamine monomer to the perfluorosulfonic acid resin is 2; and the functional regulator is trifluoromethanesulfonic acid.
[0101] The polymer matrix has a molecular structure as shown in Formula 1,
[0102]
[0103] In formula 1, x is 2.
[0104] The cross-linked proton exchange membrane has a molecular structure as shown in Formula 2,
[0105]
[0106] In formula 2, x is 2.
[0107] like Figure 2 and Figure 3 As shown, the embodiment of the present application provides a method for preparing a cross-linked proton exchange membrane, comprising:
[0108] S1. A dispersion of a perfluorosulfonic acid resin solution and an amino monomer are subjected to a grafting reaction to obtain a first reaction solution;
[0109] S2. The first reaction liquid is dried at 80°C and then calcined to obtain a polymer matrix C. 2 -SI;
[0110] S3. cross-linking the initiator, the silane coupling agent and the polymer matrix to obtain a second reaction solution;
[0111] S4. The second reaction solution is dried at 60° C. for 12 h, and then annealed and membrane stripped to obtain a coarse cross-linked proton exchange membrane;
[0112] S5. Use a functional regulator to immerse the coarse cross-linked proton exchange membrane in the medium, and then purify it to obtain a cross-linked proton exchange membrane C. x -SI x -TF.
[0113] The temperature of the grafting reaction was 25°C, and the time of the grafting reaction was 12 h.
[0114] The calcination temperature was 220°C and the calcination time was 1.5 h.
[0115] The temperature of the cross-linking reaction is 140° C., and the time of the cross-linking reaction is 12 h.
[0116] The annealing temperature is 120°C and the annealing time is 2h.
[0117] The immersion temperature was 80°C and the immersion time was 12 h.
[0118] Example 2
[0119] A cross-linked proton exchange membrane, the raw materials of the cross-linked proton exchange membrane include: a polymer matrix, a silane coupling agent, an initiator and a functional regulator, the mass ratio of the silane coupling agent to the polymer matrix is 0.03, the mass ratio of the initiator to the polymer matrix is 0.01, and the mass ratio of the functional regulator to the polymer matrix is 4:1; wherein the raw materials of the polymer matrix include N,N-dimethylethylenediamine monomer and perfluorosulfonic acid resin, the molar ratio of the N,N-dimethylethylenediamine monomer to the perfluorosulfonic acid resin is 2; and the functional regulator is phosphoric acid.
[0120] The polymer matrix has a molecular structure as shown in Formula 1,
[0121]
[0122] In formula 1, x is 2.
[0123] The cross-linked proton exchange membrane has a molecular structure as shown in Formula 3,
[0124]
[0125] In formula 3, x is 2.
[0126] like Figure 2 and Figure 3 As shown, the present embodiment provides a method for preparing a cross-linked proton exchange membrane, comprising:
[0127] S1. A dispersion of a perfluorosulfonic acid resin solution and an amino monomer are subjected to a grafting reaction to obtain a first reaction solution;
[0128] S2. The first reaction solution is dried at 80°C and then calcined to obtain a polymer matrix C2-SI;
[0129] S3. cross-linking the initiator, the silane coupling agent and the polymer matrix to obtain a second reaction solution;
[0130] S4. The second reaction solution is dried at 60° C. for 12 h, and then annealed and membrane stripped to obtain a coarse cross-linked proton exchange membrane;
[0131] S5. Use a functional regulator to immerse the coarse-grade cross-linked proton exchange membrane in, and then purify it to obtain a cross-linked proton exchange membrane Cx-SIx-PA.
[0132] The temperature of the grafting reaction was 25°C, and the time of the grafting reaction was 12 h.
[0133] The calcination temperature was 220°C and the calcination time was 1.5 h.
[0134] The temperature of the cross-linking reaction is 140° C., and the time of the cross-linking reaction is 12 h.
[0135] The annealing temperature is 120°C and the annealing time is 2h.
[0136] The immersion temperature was 80°C and the immersion time was 12 h.
[0137] Example 3
[0138] Based on the contents disclosed in Example 1, the following modifications are further made:
[0139] The grafting reaction time was 12 h.
[0140] The calcination temperature was 215°C and the calcination time was 2 h.
[0141] The temperature of the crosslinking reaction was 135°C.
[0142] The annealing temperature was 115°C.
[0143] The immersion temperature was 75°C.
[0144] Example 4
[0145] Based on the contents disclosed in Example 1, the following modifications are further made:
[0146] The grafting reaction time is 24 h.
[0147] The calcination temperature was 235°C and the calcination time was 1 h.
[0148] The temperature of the crosslinking reaction was 145°C.
[0149] The annealing temperature is 125°C.
[0150] The immersion temperature was 85°C.
[0151] Example 5
[0152] A cross-linked proton exchange membrane, the raw materials of the cross-linked proton exchange membrane include: a polymer matrix, a silane coupling agent, an initiator and a functional regulator, the mass ratio of the silane coupling agent to the polymer matrix is 0.03, the mass ratio of the initiator to the polymer matrix is =0.01, and the mass ratio of the functional regulator to the polymer matrix is 4:1; wherein the raw materials of the polymer matrix include N,N-dimethylethylenediamine monomer and perfluorosulfonic acid resin, the molar ratio of the N,N-dimethylethylenediamine monomer to the perfluorosulfonic acid resin is 2; the functional regulator is trifluoromethanesulfonic acid.
[0153] The polymer matrix has a molecular structure as shown in Formula 1,
[0154]
[0155]
[0156] In formula 1, x is 5.
[0157] The cross-linked proton exchange membrane has a molecular structure as shown in Formula 2,
[0158]
[0159] In formula 2, x is 5.
[0160] like Figure 2 and Figure 3 As shown, the embodiment of the present application provides a method for preparing a cross-linked proton exchange membrane, comprising:
[0161] S1. A dispersion of a perfluorosulfonic acid resin solution and an amino monomer are subjected to a grafting reaction to obtain a first reaction solution;
[0162] S2. The first reaction solution is dried at 80°C and then calcined to obtain a polymer matrix C5-SI;
[0163] S3. cross-linking the initiator, the silane coupling agent and the polymer matrix to obtain a second reaction solution;
[0164] S4. The second reaction solution is dried at 60° C. for 12 h, and then annealed and membrane stripped to obtain a coarse cross-linked proton exchange membrane;
[0165] S5. Use a functional regulator to immerse the coarse-grade cross-linked proton exchange membrane in, and then purify it to obtain a cross-linked proton exchange membrane C5-SIx-TF.
[0166] The temperature of the grafting reaction was 25°C, and the time of the grafting reaction was 12 h.
[0167] The calcination temperature was 220°C and the calcination time was 1.5 h.
[0168] The temperature of the cross-linking reaction is 140° C., and the time of the cross-linking reaction is 12 h.
[0169] The annealing temperature is 120°C and the annealing time is 2h.
[0170] The immersion temperature was 80°C and the immersion time was 12 h.
[0171] Comparative Example 1
[0172] Based on the contents disclosed in Example 1, the following modifications are further made:
[0173] No amino monomer or silane coupling agent is added to the dispersion of the full sulfonic acid resin solution to obtain C 5 -SA perfluorosulfonic acid membrane.
[0174] Comparative Example 2
[0175] Based on the contents disclosed in Example 1, the following modifications are further made:
[0176] Without adding silane coupling agent, C 5 -SI-TF perfluorosulfonic acid membrane.
[0177] Comparative Example 3
[0178] Based on the contents disclosed in Example 1, the following modifications are further made:
[0179] Without adding N,N-dimethylethylenediamine monomer, a silane coupling agent was added to obtain C2x-TF perfluorosulfonic acid membrane.
[0180] Related experiments and effect data:
[0181] The performance of the proton exchange membranes obtained in various embodiments and comparative examples were tested respectively, and the results are shown in Table 1.
[0182] Table 1 Performance of the proton exchange membranes obtained in various embodiments and comparative examples
[0183]
[0184] As can be seen from Table 1, a cross-linked proton exchange membrane provided in an embodiment of the present application has a sufficient amount of polyionic liquid cross-linking structure. On the one hand, a sufficient amount of polyionic liquid cross-linking structure can prevent the ionic liquid from leaching from the system under low relative humidity conditions, so as to enhance the compactness of the cross-linked proton exchange membrane while maintaining the mechanical properties of the cross-linked proton exchange membrane, thereby improving the working stability of the cross-linked proton exchange membrane under low relative humidity conditions, so as to improve the durability of the perfluorosulfonic acid proton exchange membrane. On the other hand, a sufficient amount of polyionic liquid cross-linking structure can promote the close adhesion of the cross-linked proton exchange membrane to the catalyst layer and the frame material of the sealing ring, so as to effectively prevent the peeling of the cross-linked proton exchange membrane and the catalyst layer, and delay the aging of the frame material of the sealing ring, thereby improving the service life of the perfluorosulfonic acid proton exchange membrane.
[0185] In addition, a cross-linked proton exchange membrane provided in an embodiment of the present application provides a new ionic liquid as a proton conduction carrier, which can significantly improve the proton conductivity of the cross-linked proton exchange membrane under low humidity conditions.
[0186] In addition, the embodiment of the present application provides a method for preparing a cross-linked proton exchange membrane. On the basis of a perfluorosulfonic acid proton exchange membrane, a cross-linked proton exchange membrane can be obtained using relatively simple chemical raw materials. The overall preparation method is simple, and it is a low-cost preparation process for a new type of cross-linked proton exchange membrane.
[0187] The above is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. It will be apparent to those skilled in the art that various modifications to these embodiments are possible, and the general principles defined in the present application can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to these embodiments shown in the present application, but will conform to the widest scope consistent with the principles and novel features applied for by the present application.
Claims
1. A cross-linked proton exchange membrane, characterized in that: The raw materials of the cross-linked proton exchange membrane include: a polymer matrix, a silane coupling agent, an initiator and a functional regulator, wherein the mass ratio of the silane coupling agent to the polymer matrix is ≥0.03:1, the mass ratio of the initiator to the polymer matrix is ≥0.01:1, and the mass ratio of the functional regulator to the polymer matrix is ≥1:1; Wherein, the raw materials of the polymer matrix include amino monomers and perfluorosulfonic acid resin, and the molar ratio of the amino monomers to the perfluorosulfonic acid resin is ≥2:1; The functional regulator includes sulfonate and / or phosphoric acid.
2. The cross-linked proton exchange membrane according to claim 1, characterized in that: The molar ratio of the amino monomer to the perfluorosulfonic acid resin is (2:1) to (5:1).
3. The cross-linked proton exchange membrane according to claim 1, characterized in that: The amino monomer includes N,N-dimethylethylenediamine monomer.
4. The cross-linked proton exchange membrane according to claim 1, characterized in that: The polymer matrix has a molecular structure as shown in Formula 1, In formula 1, x≥2.
5. The cross-linked proton exchange membrane according to claim 1, characterized in that: The function modulator includes trifluoromethanesulfonic acid.
6. The cross-linked proton exchange membrane according to claim 5, characterized in that: When the functional regulator is trifluoromethanesulfonic acid, the cross-linked proton exchange membrane has a molecular structure as shown in Formula 2, In formula 2, x≥2.
7. The cross-linked proton exchange membrane according to claim 1, characterized in that: When the functional regulator is phosphoric acid, the cross-linked proton exchange membrane has a molecular structure as shown in Formula 3, In formula 3, x≥2.
8. A method for preparing a cross-linked proton exchange membrane as claimed in any one of claims 1 to 7, characterized in that: The method comprises: A dispersion of a perfluorosulfonic acid resin solution and an amino monomer are subjected to a graft reaction to obtain a first reaction solution; The first reaction liquid is dried and then calcined to obtain a polymer matrix; Performing a cross-linking reaction on the initiator, the silane coupling agent and the polymer matrix to obtain a second reaction solution; The second reaction liquid is dried, and then annealed and membrane stripped to obtain a coarse-grade cross-linked proton exchange membrane; The coarse-grade cross-linked proton exchange membrane is immersed in a functional regulator, and then purified to obtain a cross-linked proton exchange membrane.
9. The method according to claim 8, characterized in that The temperature of the grafting reaction is 20° C. to 30° C., and the time of the grafting reaction is 12 h to 24 h.
10. The method according to claim 8, characterized in that The calcination temperature is 215° C. to 235° C., and the calcination time is 1 h to 2 h.
11. The method according to claim 8, characterized in that The temperature of the cross-linking reaction is 135° C. to 145° C., and the time of the cross-linking reaction is ≥12 h.
12. The method according to claim 8, characterized in that The annealing temperature is 115° C. to 125° C., and the annealing time is ≥ 2 hours.
13. The method according to claim 8, characterized in that The immersion temperature is 75° C. to 85° C., and the immersion time is ≥12 h.