Lithium battery wet recovery process
By using sodium hydroxide and sodium dodecyl phosphate in the wet recovery process of lithium batteries to generate lithium phosphate precipitation, combined with the purification treatment of flocculant and adsorbent, the problems of resource loss and environmental pollution in the prior art are solved, and the problem of resource loss and environmental pollution in the existing technology is realized. The efficient recycling and purification of lithium has promoted the sustainable development of the new energy industry.
Patent Information
- Application Number
- CN202411067334.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing wet recovery process of lithium batteries has resource losses and environmental pollution problems during the carbonation precipitation stage, and improper handling leads to resource waste.
By adding sodium hydroxide solution to adjust the pH value in the lithium battery mother liquor, adding sodium dodecyl phosphate to generate lithium phosphate precipitation, and separating and purifying using a centrifuge and filter membrane, combining the use of composite flocculant and composite adsorbent, the process of achieving the Efficient extraction and purification of lithium.
It effectively improves the recycling efficiency of lithium resources, reduces the risk of environmental pollution, realizes the recycling of resources, reduces production costs, and promotes the sustainable development of the new energy industry.
Smart Images

Figure CN119050526A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium battery recovery and resource reuse, and specifically relates to a lithium battery wet recovery process. Background Art
[0002] In 2020, my country proposed the dual carbon target at the 75th United Nations General Assembly. Against this background, the country has vigorously developed new energy vehicles. With the rapid development of new energy vehicles, power lithium-ion batteries are becoming more and more widely used. However, the life of lithium batteries is limited. The average life of automotive lithium batteries is only 3-8 years. Its large-scale use has also led to an increasing trend in its scrap volume year by year. According to forecasts, by 2030, the amount of retired lithium batteries in China will reach 3.9 million tons, and the global amount of waste lithium batteries will exceed 10 million tons. Waste lithium batteries are rich in metal elements and have extremely high value. Therefore, an efficient and environmentally friendly waste lithium battery recycling process is of great significance to promoting the sustainable development of the new energy vehicle industry and promoting resource conservation and environmental protection.
[0003] At present, the existing lithium battery recycling methods are divided into three categories: pyrometallurgical recycling, wet recycling, and biological recycling. Wet recycling is to crush and dissolve the waste lithium batteries, use chemical reagents to selectively separate the metal elements in the leaching solution, and then extract the metal elements through extraction, separation, precipitation and other methods. The recovery process mostly adopts the "reduction acid leaching-carbonation precipitation" method. There is a certain amount of loss in the "carbonation precipitation" stage, which is mainly enriched in the lithium precipitation mother liquor discharged after lithium recovery. In addition, due to improper handling, it will cause environmental pollution and waste of resources. In this regard, we propose a lithium battery wet recovery process. Summary of the invention
[0004] In view of the deficiencies in the prior art, the present invention provides a lithium battery wet recovery process to solve the above technical problems.
[0005] To achieve the above object, the present invention provides the following technical solution: a lithium battery wet recovery process, the operation steps of the recovery process are:
[0006] S1. Adding sodium hydroxide solution into the lithium battery mother liquor to adjust the pH value of the lithium mother liquor;
[0007] S2, adding sodium phosphate dodecahydrate to the adjusted lithium mother liquor, heating the reaction to generate lithium phosphate precipitate;
[0008] S3. After the reaction is completed, the lithium supernatant and the lithium phosphate precipitate in the reaction solution are separated by a centrifuge, the lithium phosphate precipitate is washed with water and then placed in an oven for drying, and then collected and stored after drying to obtain lithium extracted from the lithium battery mother liquor;
[0009] S4, adding a composite flocculant to the lithium supernatant and stirring it sufficiently to aggregate and settle the tiny particles in the lithium supernatant, placing the lithium supernatant in a high-speed refrigerated centrifuge and filtering it through a filter membrane to remove suspended matter and impurities;
[0010] S5. Put the solution after centrifugal filtration into the composite adsorbent, stir it evenly with a magnetic stirrer, put the stirred solution into a high-speed refrigerated centrifuge and filter it through a filter membrane to obtain a purified mother liquor.
[0011] Preferably, the amount of sodium hydroxide solution added in step S1 is required to adjust the pH of the lithium mother liquor to ≥12.
[0012] Preferably, in step S2, 3n(PO4 3- ): n(Li + ) was added with sodium phosphate dodecahydrate in an amount of 1.5, and the heating reaction temperature was controlled at 90°C for 1 hour.
[0013] Preferably, the formula for the chemical reaction in step S2 is:
[0014] 3Na3PO4·12H2O+2xLi+→Li3PO4
[0015] Among them, 3Na3PO4·12H2O represents sodium phosphate dodecahydrate, 2xLi+ represents lithium ions in the lithium mother solution, and Li3PO4 represents the generated lithium phosphate precipitate.
[0016] Preferably, in step S3, the speed of the centrifuge is set to 10000 r / min, the reaction time is 10 min, the lithium phosphate precipitate is washed twice, the oven temperature is set to 105° C., and the drying time is 24 h.
[0017] Preferably, after adding the composite flocculant in step S4, the mixture is reacted at a stirring speed of 100 r / min for 30 min, and the filter membrane of the filter membrane after centrifugation in a high-speed refrigerated centrifuge is 0.45 μm.
[0018] Preferably, after the composite adsorbent is added in step S5, the mixture is reacted at a stirring speed of 100 r / min for 1 hour, and the filter membrane of the filtration membrane after centrifugation in a high-speed refrigerated centrifuge is 0.45 μm.
[0019] Preferably, the purification effect of the purified mother liquor needs to be judged based on its COD removal rate.
[0020] Preferably, the COD removal rate is calculated as follows:
[0021] COD e =(COD b —COD a ) / CODb
[0022] Among them, COD e Indicates COD removal rate, unit is %, COD b Indicates the COD of the mother liquor before treatment, in mg / L, COD a Indicates the COD of the mother liquor after treatment, in mg / L.
[0023] Preferably, the lithium phosphate precipitate obtained in steps S3 and S5 and the purified mother liquor are recycled by the lithium battery production line.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] The present application uses chemical means to extract lithium from waste lithium battery mother liquor and purify the lithium battery mother liquor, thereby achieving the purpose of recycling waste resources and protecting the environment. Through a new recycling process, lithium elements can be efficiently extracted from waste lithium battery mother liquor and collected and stored in the form of lithium phosphate, thereby achieving effective recycling of lithium resources and avoiding waste of resources. By adjusting the pH value and adding composite flocculants and composite adsorbents, suspended matter, impurities and other harmful substances in the mother liquor are effectively removed, the purification effect of the mother liquor is significantly improved, and the risk of environmental pollution is reduced, which is in line with the concepts of green production and circular economy. The recovered lithium phosphate, as a high-value metal compound, can be reused in lithium battery production, reducing production costs. The efficient recycling and purification process reduces waste disposal costs and improves overall economic benefits, which is of great significance for promoting the sustainable development of the new energy industry. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a schematic diagram of the lithium battery wet recycling process. DETAILED DESCRIPTION
[0027] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] The present invention provides a technical solution: a lithium battery wet recovery process, the operation steps of the recovery process are:
[0029] S1. Add sodium hydroxide solution to the lithium battery mother liquor to adjust the pH value of the lithium mother liquor. The key to this step is to control the pH value within a specific range to optimize the efficiency and selectivity of subsequent chemical reactions, ensure the priority extraction of lithium ions, and reduce interference with other metal ions. Sodium hydroxide solution is a colorless liquid made by dissolving strong alkali sodium hydroxide in water. It is highly corrosive. When using sodium hydroxide solution, personal protective equipment including protective clothing, gloves, and glasses should be worn to avoid direct contact with the skin and eyes. Sodium hydroxide solution should be kept away from fire and heat sources to avoid combustion or explosion;
[0030] S2. Add sodium phosphate dodecahydrate to the adjusted lithium mother liquor, heat the reaction so that phosphate ions combine with lithium ions to gradually form lithium phosphate precipitate. The reaction temperature and reaction time need to be strictly controlled to ensure the purity and yield of the lithium phosphate precipitate. At the same time, monitor the pH value change in the reaction solution and make fine adjustments when necessary. Sodium phosphate dodecahydrate is also called sodium phosphate. It is an inorganic compound. Sodium phosphate dodecahydrate will decompose into disodium hydrogen phosphate and sodium hydroxide after being dissolved in water. It starts to melt when heated to 75°C and loses 11 molecules of crystal water at 100°C to form an anhydrous substance. It is easy to weather in dry air. Sodium phosphate dodecahydrate is corrosive and irritating to the skin and eyes. It needs to be moisture-proof, fire-proof and explosion-proof.
[0031] S3. After the reaction is completed, the lithium supernatant and the lithium phosphate precipitate in the reaction solution are separated by a centrifuge, the lithium phosphate precipitate is washed with water to remove impurities attached to the surface, and then placed in an oven for drying. After drying, the mixture is collected and stored to obtain lithium extracted from the lithium battery mother liquor;
[0032] S4. For the tiny particles and suspended matter in the lithium supernatant, a composite flocculant is added to the lithium supernatant and stirred sufficiently to make the flocculant uniformly dispersed in the solution. The flocculant molecules can adsorb and bridge the tiny particles, prompting them to aggregate into larger flocs, so that the tiny particles in the lithium supernatant aggregate and settle. The lithium supernatant is placed in a high-speed refrigerated centrifuge to utilize the change in the material properties at low temperature and the effect of centrifugal force to further accelerate the sedimentation of particles and remove suspended matter, and then filtered through a filter membrane to effectively intercept and remove suspended matter and impurities;
[0033] S5. In order to further improve the purity of the mother liquor, the solution after centrifugal filtration is placed in a composite adsorbent. The composite adsorbent has the characteristics of strong selectivity and large adsorption capacity, and can specifically adsorb the residual impurities and incompletely precipitated metal ions in the solution. A magnetic stirrer is used to stir evenly to make the adsorbent and the solution fully contact to achieve efficient adsorption. After the adsorption is completed, the stirred solution is placed in a high-speed refrigerated centrifuge and filtered through a filter membrane to obtain a purified mother liquor. The final mother liquor has an extremely low impurity content, which provides high-quality raw materials for subsequent lithium extraction or recycling.
[0034] Furthermore, the amount of sodium hydroxide solution added in step S1 needs to adjust the pH of the lithium mother liquor to ≥12. The purpose of adjusting the pH of the lithium mother liquor to pH ≥12 is to create a strong alkaline environment. The strong alkaline environment is conducive to the formation of lithium phosphate precipitation in the subsequent steps. Under alkaline conditions, lithium phosphate has a higher solubility and product constant, which means that in a strong alkaline solution, phosphate ions and lithium ions are more likely to combine to form lithium phosphate precipitates. In the process of adjusting the pH value, it is necessary to pay close attention to the color and smell of the lithium mother liquor so as to promptly discover and deal with possible abnormal situations.
[0035] Furthermore, in step S2, 3n(PO4 3- ): n(Li + ) is added with sodium phosphate dodecahydrate in an amount of 1.5, the temperature of the heating reaction is controlled at a constant temperature of 90°C, and the reaction time is 1h. The dosage ratio of sodium phosphate dodecahydrate is the conclusion drawn after rigorous experiments. When the dosage ratio of sodium phosphate dodecahydrate is increased from 1.0 to 1.5, Li + The yield was improved most significantly, with the extraction rate increasing from 81.4% to 99.5%. However, when the concentration of sodium phosphate increased from 1.5 to 3.0, the Li + The yield remains basically unchanged, but the mass of the precipitate is constantly increasing, indicating that other elements in the lithium-containing mother liquor are constantly precipitating, resulting in an increasing impurity content in the product obtained by lithium precipitation, a decrease in product purity, and an increasing content of total phosphorus in the mother liquor. Therefore, considering that the residual phosphorus in the mother liquor should not be too high, it is best to control the amount of sodium phosphate dodecahydrate in the solution to 3n(PO43-):n(Li+)≤1.5.
[0036] Furthermore, the formula for the chemical reaction in step S2 is:
[0037] 3Na3PO4·12H2O+2xLi+→Li3PO4
[0038] Among them, 3Na3PO4·12H2O represents sodium phosphate dodecahydrate, 2xLi+ represents lithium ions in the lithium mother solution, and Li3PO4 represents the generated lithium phosphate precipitate.
[0039] Furthermore, in step S3, the speed of the centrifuge is set to 10000r / min to generate a strong centrifugal force, which enables the solid particles and the liquid part in the reaction liquid to be quickly and effectively separated, thereby improving the purity of lithium phosphate. The reaction time is 10min. During this time period, the centrifuge can achieve the best state of solid-liquid separation. Too short a reaction time will lead to incomplete separation, while too long a time will increase energy consumption without significantly improving the quality of the precipitate. The lithium phosphate precipitate is washed twice to remove impurities and unreacted ions attached to the surface of the precipitate, and is placed in an oven at a temperature of 105°C and a drying time of 24h to ensure that the precipitate can be fully dried and improve stability and storage performance.
[0040] Furthermore, after adding the composite flocculant in step S4, the mixture is reacted at a stirring speed of 100 r / min for 30 minutes. After centrifugation in a high-speed refrigerated centrifuge, the filter membrane of the filter membrane is 0.45 μm. The composite flocculant is a mixture of various polymer compounds, and has excellent flocculation and sedimentation properties. It can quickly aggregate tiny particles and colloid-like suspended solids in the solution into larger flocs for subsequent separation. During the centrifugation process, the temperature is controlled at a low temperature, which is beneficial to reducing the content of dissolved oxygen and other volatile substances in the solution. The 0.45 μm filter membrane can effectively intercept tiny particles and colloid substances in the solution. During the filtration process, the flow rate and pressure need to be maintained to ensure that the filter membrane is not blocked and the filtration efficiency is not affected.
[0041] Furthermore, after adding the composite adsorbent in step S5, the mixture is reacted at a stirring speed of 100 r / min for 1 hour. After centrifugation in a high-speed refrigerated centrifuge, the filter membrane used for filtration is 0.45 μm. The composite adsorbent is a highly efficient adsorption material that can selectively adsorb impurity ions, organic matter and other unnecessary components in the solution to improve the purity of the solution. During the stirring process, the composite adsorbent will gradually adsorb impurities in the solution, making the solution clearer, thereby ensuring that the final purified mother liquor has extremely high purity.
[0042] Furthermore, the purification effect of the mother liquor after purification needs to be judged based on its COD removal rate. By comparing the COD values of the mother liquor before and after treatment, the removal effect of organic pollution during the purification process can be intuitively understood. The COD removal rate directly reflects the effectiveness and stability of the purification process.
[0043] Furthermore, the COD removal rate calculation method is:
[0044] COD e =(COD b —COD a ) / COD b
[0045] Among them, CODe Indicates COD removal rate, unit is %, COD b Indicates the COD of the mother liquor before treatment, in mg / L, COD a Indicates the COD of the mother liquor after treatment, in mg / L.
[0046] Furthermore, the lithium phosphate precipitate obtained in steps S3 and S5 and the purified mother liquor are recycled by the lithium battery production line. The lithium phosphate precipitate is not only an important form of lithium recovery, but also plays a key role in the manufacture of lithium batteries due to its unique chemical properties. After fine treatment and purification, these lithium phosphate precipitates can be used as one of the raw materials for preparing positive electrode materials and directly applied to the production process of lithium batteries. By reintroducing them into the production line, not only the dependence on primary mineral resources is reduced, but also the production cost is reduced and the resource utilization efficiency is improved. The mother liquor can be used as a solvent or reaction medium in multiple links of lithium battery production. It can be used as a basic component of the electrolyte to participate in the regulation of the electrochemical reaction inside the battery. It can also be used as a cleaning fluid for cleaning and pretreatment of battery components.
[0047] Example 1
[0048] A1. Add sodium hydroxide solution into the lithium battery mother liquor to adjust the pH value of the lithium mother liquor;
[0049] A2, adding sodium phosphate dodecahydrate to the adjusted lithium mother liquor in an amount of 3n(PO43-):n(Li+)=1.0, heating the reaction to generate lithium phosphate precipitate;
[0050] A3. After the reaction is completed, use a centrifuge to separate the lithium supernatant and lithium phosphate precipitate in the reaction solution, wash the lithium phosphate precipitate with water and then put it into an oven for drying. After drying, collect and store it to obtain the lithium extracted from the lithium battery mother liquor and weigh it.
[0051] Example 2
[0052] A1. Add sodium hydroxide solution into the lithium battery mother liquor to adjust the pH value of the lithium mother liquor;
[0053] A2, adding sodium phosphate dodecahydrate to the adjusted lithium mother liquor in an amount of 3n(PO43-):n(Li+) of 1.5, heating the reaction to generate lithium phosphate precipitate;
[0054] A3. After the reaction is completed, use a centrifuge to separate the lithium supernatant and lithium phosphate precipitate in the reaction solution, wash the lithium phosphate precipitate with water and then put it into an oven for drying. After drying, collect and store it to obtain the lithium extracted from the lithium battery mother liquor and weigh it.
[0055] Example 3
[0056] A1. Add sodium hydroxide solution into the lithium battery mother liquor to adjust the pH value of the lithium mother liquor;
[0057] A2, adding sodium phosphate dodecahydrate to the adjusted lithium mother liquor in an amount of 3n(PO43-):n(Li+)=2, heating the reaction to generate lithium phosphate precipitate;
[0058] A3. After the reaction is completed, use a centrifuge to separate the lithium supernatant and lithium phosphate precipitate in the reaction solution, wash the lithium phosphate precipitate with water and then put it into an oven for drying. After drying, collect and store it to obtain the lithium extracted from the lithium battery mother liquor and weigh it.
[0059] Example 4
[0060] A1. Add sodium hydroxide solution into the lithium battery mother liquor to adjust the pH value of the lithium mother liquor;
[0061] A2, adding sodium phosphate dodecahydrate to the adjusted lithium mother liquor in an amount of 3n(PO43-):n(Li+) of 2.5, heating the reaction to generate lithium phosphate precipitate;
[0062] A3. After the reaction is completed, use a centrifuge to separate the lithium supernatant and lithium phosphate precipitate in the reaction solution, wash the lithium phosphate precipitate with water and then put it into an oven for drying. After drying, collect and store it to obtain the lithium extracted from the lithium battery mother liquor and weigh it.
[0063] Example 5
[0064] A1. Add sodium hydroxide solution into the lithium battery mother liquor to adjust the pH value of the lithium mother liquor;
[0065] A2, adding sodium phosphate dodecahydrate to the adjusted lithium mother liquor in an amount of 3n(PO43-):n(Li+)=3, heating the reaction to generate lithium phosphate precipitate;
[0066] A3. After the reaction is completed, use a centrifuge to separate the lithium supernatant and lithium phosphate precipitate in the reaction solution, wash the lithium phosphate precipitate with water and then put it into an oven for drying. After drying, collect and store it to obtain the lithium extracted from the lithium battery mother liquor and weigh it.
[0067] Table 1 below is a table showing the yield of lithium phosphate precipitate extracted from 50 ml lithium-containing mother liquor in different embodiments.
[0068]
[0069]
[0070] Table 1
[0071] According to experiments, the lithium phosphate precipitation extraction effect is best when the dosage ratio of sodium phosphate dodecahydrate is 3n(PO43-):n(Li+)≤1.5.
[0072] On the basis of Example 2, the separated lithium supernatant was further tested. Four groups of 50 ml mother liquor after lithium precipitation were taken into a 100 mL beaker, and a 20% PFS solution, a 0.1% PAM anion solution and a composite flocculant were prepared. The experimental steps were as follows:
[0073] Example 6
[0074] Add 1 ml of PFS solution to the lithium supernatant and stir it thoroughly at a speed of 100 r / min for 10 minutes. Then add 1 ml of PAM solution and stir it thoroughly at a speed of 100 r / min for 10 minutes to make the tiny particles in the lithium supernatant aggregate and settle. Put the lithium supernatant into a high-speed refrigerated centrifuge, adjust the pH value to 7 after centrifugal filtration, and then filter it through a filter membrane to remove suspended matter and impurities. Measure its COD after flocculation.
[0075] Example 7
[0076] Add 2 ml of PFS solution to the lithium supernatant and stir it thoroughly at a speed of 100 r / min for 10 minutes. Then add 2 ml of PAM solution and stir it thoroughly at a speed of 100 r / min for 10 minutes to make the tiny particles in the lithium supernatant aggregate and settle. Put the lithium supernatant into a high-speed refrigerated centrifuge, adjust the pH value to 7 after centrifugal filtration, and then filter it through a filter membrane to remove suspended matter and impurities. Measure its COD after flocculation.
[0077] Example 8
[0078] Add 1 ml of composite flocculant to the lithium supernatant and stir it at a speed of 100 r / min for 30 minutes to allow the tiny particles in the lithium supernatant to aggregate and settle. Put the lithium supernatant into a high-speed refrigerated centrifuge and filter it through a membrane to remove suspended matter and impurities. Measure its COD after flocculation.
[0079] Example 9
[0080] Add 2 ml of composite flocculant to the lithium supernatant and stir it at a speed of 100 r / min for 30 minutes to make the tiny particles in the lithium supernatant aggregate and settle. Put the lithium supernatant into a high-speed refrigerated centrifuge and filter it through a filter membrane to remove suspended matter and impurities. Measure its COD after flocculation.
[0081] Table 2 below is a table showing the experimental results of different flocculant addition amounts in different embodiments.
[0082] Group COD after flocculation (mg / L) COD removal rate (%) Example 1 28895 17.23 Example 2 27315 21.76 Example 3 17155 45.98 Example 4 8575 73.00
[0083] Table 2
[0084] According to the experiment, the flocculation effect of the composite flocculant is much better than that of PFS solution and PAM solution, and the flocculation effect is greatly improved with the increase of the dosage of the composite flocculant.
[0085] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0086] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A lithium battery wet recovery process, characterized in that: The operating steps of the recycling process are: S1. Adding sodium hydroxide solution into the lithium battery mother liquor to adjust the pH value of the lithium mother liquor; S2, adding sodium phosphate dodecahydrate to the adjusted lithium mother liquor, heating the reaction to generate lithium phosphate precipitate; S3. After the reaction is completed, the lithium supernatant and the lithium phosphate precipitate in the reaction solution are separated by a centrifuge, the lithium phosphate precipitate is washed with water and then placed in an oven for drying, and then collected and stored after drying to obtain lithium extracted from the lithium battery mother liquor; S4, adding a composite flocculant to the lithium supernatant and stirring it sufficiently to aggregate and settle the tiny particles in the lithium supernatant, placing the lithium supernatant in a high-speed refrigerated centrifuge and filtering it through a filter membrane to remove suspended matter and impurities; S5. Put the solution after centrifugal filtration into the composite adsorbent, stir it evenly with a magnetic stirrer, put the stirred solution into a high-speed refrigerated centrifuge and filter it through a filter membrane to obtain a purified mother liquor.
2. The lithium battery wet recovery process according to claim 1, characterized in that: The amount of sodium hydroxide solution added in step S1 is required to adjust the pH of the lithium mother liquor to ≥12.
3. The lithium battery wet recovery process according to claim 1, characterized in that: In step S2, press 3n(PO4 3- ): n(Li + ) was added with sodium phosphate dodecahydrate in an amount of 1.5, and the heating reaction temperature was controlled at 90°C for 1 hour.
4. The lithium battery wet recovery process according to claim 1, characterized in that: The formula for the chemical reaction in step S2 is: 3Na3PO4·12H2O+2xLi+→Li3PO4 Among them, 3Na3PO4·12H2O represents sodium phosphate dodecahydrate, 2xLi+ represents lithium ions in the lithium mother solution, and Li3PO4 represents the generated lithium phosphate precipitate.
5. The lithium battery wet recovery process according to claim 1, characterized in that: In step S3, the speed of the centrifuge is set to 10000 r / min, the reaction time is 10 min, the lithium phosphate precipitate is washed twice, the oven temperature is set to 105° C., and the drying time is 24 h.
6. The lithium battery wet recovery process according to claim 1, characterized in that: After adding the composite flocculant in step S4, the mixture was stirred at a speed of 100 r / min for 30 min, and the filter membrane was filtered after centrifugation in a high-speed refrigerated centrifuge with a 0.45 μm filter membrane.
7. The lithium battery wet recovery process according to claim 1, characterized in that: After the composite adsorbent is added in step S5, the mixture is reacted at a stirring speed of 100 r / min for 1 hour, and the filter membrane of the filter membrane after centrifugation in a high-speed refrigerated centrifuge is 0.45 μm.
8. The lithium battery wet recovery process according to claim 1, characterized in that: The purification effect of the mother liquor after purification needs to be judged based on its COD removal rate.
9. The lithium battery wet recovery process according to claim 8, characterized in that: The COD removal rate calculation method is: CODE e =(CODE b -CODE a ) / CODE b Among them, COD e Indicates COD removal rate, unit is %, COD b Indicates the COD of the mother liquor before treatment, in mg / L, COD a Indicates the COD of the mother liquor after treatment, in mg / L.