Heating film, atomizing core and atomizing device
By using an isometric crystal structure iron-based alloy film, the dry burning and wet burning performance problems of metal heating film in electronic atomization components are solved, cost reduction and performance improvement are achieved, the defects of columnar crystal structure are overcome, and the more Stable heating performance.
Patent Information
- Application Number
- CN202310636422.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-12-03
AI Technical Summary
In existing electronic atomization components, metal heating films are prone to dry burning and electrochemical corrosion during heating, resulting in failure, and are costly, making it difficult to meet the performance requirements of dry burning and wet burning resistance.
The iron-based alloy film has an equiaxed crystal structure, which is prepared by physical vapor deposition and heat treatment to form an austenite crystal form with a face-centered cubic structure, which overcomes the defects of the columnar crystal structure and reduces costs.
The iron-based alloy films show strong resistance in high-temperature oxidation and electrochemical corrosion. The resistance changes remain stable in dry and wet calcination tests, with a longer life and a significantly reduced cost, exceeding the performance of platinum films.
Smart Images

Figure CN119054954A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a heating film, an electronic cigarette atomization component and an electronic cigarette, and belongs to the technical field of electronic cigarettes. Background Art
[0002] New electronic atomization components mostly use thin-film heating films to replace traditional thick films. The advantages of thin-film heating films are good material consistency, thin film thickness, and they will not fill the micropores on the heating surface of the porous substrate, which will not affect the transmission speed of the smoke oil and can achieve higher atomization efficiency. Commonly used metal resistance heating films are mainly low-resistivity metal materials such as Ag, Cu, and Al.
[0003] Electronic atomization components face the following problems during use: On the one hand, if there is insufficient liquid supply during the heating and atomization process, the heating film will dry-burn and the temperature may even reach over 1000°C, which can easily lead to the failure of the heating film due to dry-burning; on the other hand, atomization is achieved by heating the heating film with electricity (the potential difference is usually around 3-4V). At the same time, due to the wide variety of e-cigarette liquids, the ingredients in them also contain some corrosive media. Therefore, during the atomization process, the metal heating film is prone to electrochemical corrosion, which leads to corrosion failure of the heating film. Therefore, the requirements of electronic atomization components for metal heating films are very strict. They need to meet the requirements of both dry-burning and wet-burning performance. Commonly used metal heating films are difficult to meet the requirements.
[0004] At present, the heating film system that fully meets the requirements is mainly based on the precious metal platinum, but the cost of this material is extremely high, and there is a great cost resistance to the subsequent mass production and promotion of heating bodies. Therefore, it is urgent to develop a low-cost heating film based on base metal materials and meet the performance requirements of the heating film of the electronic atomization component for resistance to dry burning and wet burning. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a heating film based on an iron-based alloy, reduce the production cost of the heating film, and the film can meet the performance requirements of the heating film of the electronic atomization component for resistance to dry burning and wet burning. The present invention is implemented by the following technical solutions:
[0006] A heating film is an iron-based alloy film having an equiaxed crystal structure.
[0007] Optionally, the heating film has a thickness of 0.5-3 um.
[0008] Optionally, the iron-based alloy film is a stainless steel film.
[0009] Optionally, the iron-based alloy film comprises the following components by mass fraction:
[0010] Fe: 61-72%, Cr: 16-20%, Ni: 10-15%, Mo: 2-4%;
[0011] Preferably, the iron-based alloy film comprises the following components by mass fraction:
[0012] Fe: 67~72%, Cr: 16-18%, Ni: 10-12%, Mo~2-3%;
[0013] Preferably, the iron-based alloy film comprises the following components by mass fraction:
[0014] Fe: 61~67%, Cr~18-20%, Ni~12-15%, Mo~3-4%;
[0015] Optionally, the iron-based alloy film has a content of other elements less than 1% by mass.
[0016] Optionally, the iron-based alloy film has an austenite crystal form with a face-centered cubic structure;
[0017] The iron-based alloy film is measured by CuKα radiation and θ-2θ scanning. The iron-based alloy film shows an X-ray diffraction spectrum, and the X-ray diffraction peak intensity ratio of the crystal (111) plane and the (200) plane is (1-3.5):1.
[0018] Optionally, the iron-based alloy film has no grain boundaries along the thickness direction.
[0019] The present application also proposes a method for preparing the above-mentioned heating film, comprising the following steps:
[0020] Step 1) preparing an iron-based alloy film by physical vapor deposition;
[0021] Step 2) heat-treating the iron-based alloy film described in step 1) to form an equiaxed crystal structure, thereby obtaining the heat-generating film.
[0022] Optionally, in step 1), the iron-based alloy film is prepared by physical vapor deposition co-sputtering of a single metal target or physical vapor deposition sputtering of an alloy target.
[0023] Optionally, the heat treatment method in step 2) is to heat the -2 The mixture was kept at a vacuum degree of 1.000 Pa and a temperature of 600-800°C for 30 minutes, and then cooled.
[0024] Optionally, after the insulation in step 2) is completed, the furnace is cooled.
[0025] Optionally, in step 2), in 3*10 -4Pa~5*10 -2 Pa vacuum degree and keep warm at 700-800℃ for 30-120min.
[0026] The present application also proposes an electronic cigarette atomization core, wherein the electronic cigarette atomization core comprises the above-mentioned heating film.
[0027] Optionally, the atomization core includes a heating substrate, the heating substrate is provided with the heating film, and the heating film is provided with a protective film.
[0028] The present application also proposes an atomization device, which includes the above-mentioned heating film and / or the above-mentioned atomization core.
[0029] Compared with the prior art, the present invention has the following technical effects:
[0030] The present invention proposes a heating film, which is an iron-based alloy film, and the iron-based alloy film has an equiaxed crystal structure. Iron-based alloys such as stainless steel have certain corrosion resistance and oxidation resistance, and can be used to make heating materials. However, since iron-based alloys such as stainless steel blocks usually have a columnar crystal structure when prepared into films, grow along a specific crystal direction, and have a large defect content, when used as heating films for dry and wet burning tests, it is easy to oxidize or corrode along the columnar crystal boundaries, resulting in excessive increase in resistance and a short life. The iron-based alloy heating film in the present invention has an equiaxed crystal structure, the grain growth is isotropic, and the grains do not have obvious orientation, which overcomes the disadvantage of short service life of heating films with columnar crystal structures, and can meet the performance requirements of the heating film resistant to dry and wet burning during the use of the atomization core, and compared with platinum heating films, the cost is significantly reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a cross-sectional morphology diagram of the heating film of Example 1;
[0032] Figure 2 This is a cross-sectional morphology diagram of the heating film of Example 2;
[0033] Figure 3 This is a cross-sectional morphology of the heating film of Comparative Example 1;
[0034] Figure 4 This is the cross-sectional morphology of the heating film of comparative example 2
[0035] Figure 5 The following are the X-ray diffraction patterns of the heating films of various embodiments and comparative examples. DETAILED DESCRIPTION
[0036] Iron-based alloys such as stainless steel have certain corrosion resistance and oxidation resistance, and can be used to make heating materials. However, since stainless steel blocks usually have a columnar crystal structure when prepared into films, they grow along a specific crystal direction and have a large defect content. When used as heating films for dry and wet burning tests, they are prone to oxidation or corrosion along the columnar crystal boundaries, resulting in excessive increase in resistance and a short life. The present invention proposes a heating film, which is an iron-based alloy film, and the iron-based alloy film has an equiaxed crystal structure. In this equiaxed crystal structure film, the grains grow is isotropically, and there is no obvious orientation of the grains, which overcomes the disadvantage of the low life of the columnar crystal structure heating film. And compared with platinum heating films, the cost is significantly reduced. In a specific embodiment, the iron-based alloy film is an equiaxed crystal structure.
[0037] In an optional embodiment, the heating film has a thickness of 0.5-3 um. For example, the film thickness is 0.5 um, 1 um, 1.5 um, 2 um, 2.5 um, 3 um, 3.5 um, 4 um, 4.5 um, 5 um.
[0038] In an optional embodiment, the iron-based alloy film is a stainless steel film. In an optional embodiment, the iron-based alloy film comprises the following components by mass fraction: Fe: 61-72%, Cr: 16-20%, Ni: 10-15%, Mo: 2-4%. Preferably, the iron-based alloy film comprises by mass fraction: Fe: 67-72%, Cr: 16-18%, Ni: 10-12%, Mo~2-3%. Preferably, the iron-based alloy film comprises by mass fraction: Fe: 61-67%, Cr~18-20%, Ni~12-15%, Mo~3-4%.
[0039] In an optional embodiment, the iron-based alloy film has an austenite crystal form with a face-centered cubic structure; the iron-based alloy film is measured using CuKα radiation and θ-2θ scanning, and the iron-based alloy film exhibits an X-ray diffraction pattern, and the X-ray diffraction peak intensity ratio of the crystal (111) plane to the (200) plane is (1-3.5): 1. In an optional embodiment, the iron-based alloy film has no grain boundaries along the thickness direction. It has strong resistance to high temperature oxidation and electrochemical corrosion.
[0040] The present application also proposes a method for preparing the above-mentioned heating film, comprising the following steps:
[0041] Step 1) preparing an iron-based alloy film by physical vapor deposition;
[0042] Step 2) heat-treating the iron-based alloy film described in step 1) to form an equiaxed crystal structure, thereby obtaining the heating film. The preparation method adopts a physical vapor deposition method to prepare a film with a thickness of 0.5-3um, and then heat-treating the film to obtain the heating film. The prepared heating film has uniform and dense thickness, strong resistance to high temperature oxidation and electrochemical corrosion, and low manufacturing cost.
[0043] In an optional embodiment, in step 1), the iron-based alloy film is prepared by physical vapor deposition co-sputtering of a single metal target or physical vapor deposition sputtering of an alloy target.
[0044] In an optional embodiment, the heat treatment method in step 2) is to heat the -3 Pa vacuum, 700-800°C for 30 min, and then cooled. In an optional embodiment, the heat treatment is performed at 3*10 -4 Pa~5*10 -2 Pa vacuum degree and keep warm at 700-800℃ for 30-120min.
[0045] The present application also proposes an electronic cigarette atomizer core, wherein the electronic cigarette atomizer component includes the above-mentioned heating film. In an optional embodiment, the atomizer core includes a heating substrate, the heating substrate is provided with the heating film, and the heating film is provided with a protective film.
[0046] The present application also proposes an atomization device, which includes at least one of the above-mentioned heating film and the above-mentioned electronic cigarette atomization core.
[0047] The atomizer core and atomizer device using the above-mentioned heating film can resist high-temperature oxidation to a certain extent in the dry-burning test of the heating film, and ensure that the resistance value increases by less than 20% in the 8.5W dry-burning test; in the wet-burning test of the heating film, it can also improve the film's resistance to electrochemical corrosion, ensuring that the resistance value remains stable under long-term power-on and smoke oil environment.
[0048] The following examples are provided only for the purpose of illustrating the present invention in more detail. Therefore, according to the purpose of the present invention, it is obvious to those skilled in the art that the examples should not be construed as limiting the scope of the present invention. The materials involved in the examples are all commercially available products.
[0049] The test method for resistance change in each embodiment and comparative example is as follows: dry-burning test resistance change method: first test the initial resistance R0 of the heating film, the heating film is energized at a constant power of 7.5W for 3s and then stopped for 8s, and dry-burned in the air for 10 cycles. The resistance R10 of the heating film after dry-burning for 10 cycles can be calculated, and the resistance change rate ΔR before and after dry-burning can be calculated as (R10-R0) / R0, and the resistance change rate ΔR is required to be less than 20%.
[0050] Wet burning test resistance change method: load the heating element with e-liquid, test the initial resistance R0 after loading, select a 7.5w constant power battery, power on for 3s and then stop for 15s, test the resistance Rx of the heating film of the cartridge after 150 puffs, calculate the resistance change rate ΔR before and after wet burning = (Rx-R0) / R0, and the resistance change rate ΔR is required to be less than 20%.
[0051] The cross-sectional morphology of the heating film in each embodiment and comparative example is obtained by breaking the sample to obtain a natural cross section, sputtering a conductive layer of Pt for 20 seconds, and observing with a FEI Apreo C Lovac field emission scanning electron microscope.
[0052] X-ray diffraction patterns in various embodiments and comparative examples: Phase analysis was performed using a Rigaku Miniflex X-ray diffractometer (XRD) with a scanning range of 30° to 90°.
[0053] The strawberry-watermelon ice fruit-flavored e-liquid in each embodiment is: strawberry-watermelon flavored e-liquid (40 mg) produced by Shenzhen Yupeng Technology Co., Ltd.
[0054] Example 1
[0055] Preparation of heating film:
[0056] Step 1) A magnetron sputtering device is used on a heating substrate to prepare an iron-based alloy film by direct current DC sputtering of an alloy target, wherein the iron-based alloy film comprises, by mass fraction, Fe~70%, Cr~16.5%, Ni~10.5%, and Mo~2.5%, and the alloy contains inevitable impurities such as C, Si, and P, and the total mass percentage of impurities is less than 1%. The heating substrate is an array pore structure with a porosity of 20%.
[0057] Step 2) The iron-based alloy film prepared above is heat-treated at 800°C for 30 minutes under a vacuum degree of 3*10-3Pa, and then cooled in the furnace to obtain a heating substrate covered with a heating film.
[0058] A 100nm Al2O3 protective film is deposited on the surface of the heating film, and then assembled into a heating component. The effective heating area of the heating film is 3.5mm 2(This value does not take into account porosity). And further assembled into an electronic cigarette. The assembled electronic cigarette was subjected to dry burning and wet burning tests, and the test results were:
[0059] The dry-burning capacity of the heating film: 8.5W dry-burning 10 puffs resistance change is 18% (8.5W constant power on for 3s and stop for 8s dry-burning in the air); the wet-burning capacity of the heating film: 7.5W puffing 800 puffs of strawberry watermelon ice fruit flavored e-liquid resistance change = 14.5% (7.5W puffing for 3s and stop for 15s, capacity 55mL).
[0060] The cross-sectional morphology of the heating film is as follows Figure 1 As shown: the film thickness is 1600nm. The film is dense, block-like equiaxed crystals, with no obvious grain boundaries and few defects. The film was tested by XRD, and the x-ray diffraction spectrum of the heating film was analyzed to be an austenite crystal with a face-centered cubic structure. Figure 5 As shown, the test results show that there is no obvious grain growth orientation in the film. Using CuKα radiation and θ-2θ scanning for measurement, the iron-based alloy film shows an X-ray diffraction pattern, and the X-ray diffraction peak intensity ratio of the crystal (111) plane to the (200) plane is 1.87.
[0061] Example 2
[0062] Preparation of heating film:
[0063] Step 1) A magnetron sputtering device is used on a heating substrate to prepare an iron-based alloy film by direct current DC sputtering of an alloy target, wherein the iron-based alloy film comprises, by mass fraction, Fe~63.5%, Cr~19%, Ni~13.5%, and Mo~3.5%, and the alloy contains inevitable impurities such as C, Si, and P, and the total mass percentage of impurities is less than 1%. The heating substrate is an array pore structure with a porosity of 20%.
[0064] Step 2) The iron-based alloy film prepared above is heat-treated at 800°C for 30 minutes under a vacuum of 3*10-3Pa, and then cooled in the furnace to obtain a heating substrate covered with a heating film.
[0065] A 100nm Al2O3 protective film is deposited on the surface of the heating film, and then assembled into a heating component. The effective heating area of the heating film is 3.5mm 2 (This value does not take into account porosity). And further assembled into an electronic cigarette. The assembled electronic cigarette was subjected to dry burning and wet burning tests, and the test results were:
[0066] The dry burning capacity of the heating element: 8.5W dry burning 10 puffs resistance change = 18% (8.5W constant power on 3s and stop 8s dry burning in the air); wet burning capacity: 7.5W puffing strawberry watermelon ice fruit flavored e-liquid 800 puffs resistance change = 10% (7.5W puffing 3s and stop 15s, capacity 55mL).
[0067] The cross-sectional morphology of the heating film is as follows Figure 2 As shown: the film thickness is 1700nm. The film is dense, block-like equiaxed crystals, no obvious grain boundaries, and few defects. XRD test of the film, such as Figure 5 As shown, the X-ray diffraction pattern of the heating film is an austenite crystal with a face-centered cubic structure, and there is no obvious grain growth orientation. Using CuKα radiation and θ-2θ scanning for measurement, the iron-based alloy film shows an X-ray diffraction pattern, and the X-ray diffraction peak intensity ratio of the crystal (111) plane to the (200) plane is 2.63.
[0068] Example 3
[0069] A heating film is prepared according to the method in Example 1, wherein the iron-based alloy film contains by mass fraction: Fe~61%, Cr~19.5%, Ni~15%, Mo~4%, and the rest are inevitable impurities such as C, Si, P, and the total mass percentage of impurities is less than 1%. The other steps are the same as in Example 1. Dry burning and wet burning tests were carried out, and the test results are as follows: Dry burning capacity: 8.5W dry burning 10 puffs resistance change = 19% (8.5W constant power on 3s stop 8s dry burning in air); wet burning capacity: Strawberry Watermelon Ice Fruit Flavored E-liquid 7.5W puff 800 puffs resistance change = 9% (7.5W puff 3s stop 15s, capacity 55mL).
[0070] Example 4
[0071] A heating film is prepared according to the method in Example 1, wherein the iron-based alloy film contains by mass fraction: Fe~71%, Cr~16.5%, Ni~10%, Mo~2%, and the rest are inevitable impurities such as C, Si, P, and the total mass percentage of impurities is less than 1%. The other steps are the same as in Example 1. Dry burning and wet burning tests were carried out, and the test results are as follows: Dry burning capacity: 8.5W dry burning 10 puffs resistance change = 9% (8.5W constant power on for 3s and stop for 8s dry burning in the air); Wet burning capacity: Strawberry Watermelon Ice Fruit Flavored E-liquid 7.5W puffs resistance change = 19% (7.5W puffs for 3s and stop for 15s, capacity 55mL).
[0072] Comparative Example 1
[0073] Preparation of heating film:
[0074] The magnetron sputtering equipment is used on the heating substrate to prepare the iron-based alloy film by DC sputtering alloy target. The iron-based alloy film contains Fe~70%, Cr~16.5%, Ni~10.5%, Mo~2.5% by mass fraction. The alloy contains inevitable impurities such as C, Si, P, and the total impurity mass percentage is less than 1%. The heating substrate is an array pore structure with a porosity of ~20%.
[0075] A 100nm Al2O3 protective film is deposited on the surface of the heating film, and then assembled into a heating component. The effective heating area of the heating film is 3.5mm 2 (This value does not take into account porosity). And further assembled into an electronic cigarette. The assembled electronic cigarette was subjected to dry burning and wet burning tests, and the test results were:
[0076] The dry-burning capacity of the heating film: 7.5W dry-burning 10 puffs resistance change = 90%, 6.5W dry-burning 10 puffs resistance change = 19% (7.5w / 6.5W constant power power on 3s and stop 8s dry burning in the air); wet-burning capacity: 7.5W strawberry watermelon ice fruit flavored e-liquid puff 600 puffs resistance change = 15%, 800 puffs resistance change = 35% (7.5W puff 3s and stop 15s, capacity 55mL).
[0077] The cross-sectional morphology of the heating film is as follows Figure 3 As shown: the film thickness is 1700nm. The film is dense, and some areas show obvious columnar crystal characteristics and obvious grain boundaries. XRD test of the film, such as Figure 5 As shown, the X-ray diffraction analysis of the heating film includes austenite crystal form with a face-centered cubic structure and ferrite crystal form with a body-centered cubic structure. The measurement is carried out using CuKα radiation and θ-2θ scanning. The iron-based alloy film exhibits an X-ray diffraction pattern, in which the peak intensity ratio of the (111) plane to the (200) plane in the austenite crystal form with a face-centered cubic structure is 4.
[0078] Comparative Example 2
[0079] Preparation of heating film:
[0080] The iron-based alloy film is prepared by direct current DC sputtering alloy target material using magnetron sputtering equipment on the heating substrate. The iron-based alloy film contains Fe~63.5%, Cr~19%, Ni~13.5%, Mo~3.5% by mass fraction. The alloy contains inevitable impurities such as C, Si, P, etc., and the total mass percentage of impurities is less than 1%. The heating substrate is an array pore structure with a porosity of ~20%.
[0081] A 100nm Al2O3 protective film is deposited on the surface of the heating film, and then assembled into a heating component. The effective heating area of the heating film is 3.5mm 2(This value does not take into account porosity). And further assembled into an electronic cigarette. The assembled electronic cigarette was subjected to dry burning and wet burning tests, and the test results were:
[0082] The dry-burning capacity of the heating element: 6.5W dry-burning 10 puffs resistance change = 83%, 5.5W dry-burning 10 puffs resistance change = 18% (6.5w / 5.5W constant power power on 3s and stop 8s dry burning in the air); wet-burning capacity: 7.5W strawberry watermelon ice fruit flavored e-liquid puff 300 puffs resistance change = 17%, 400 puffs resistance change = 38% (7.5W puff 3s and stop 15s, capacity 55mL).
[0083] The cross-sectional morphology of the heating film is as follows Figure 4 As shown: the film thickness is 1750nm. The cross-sectional morphology of the heating film shows obvious columnar crystal characteristics, and the columnar crystal boundary runs through the height direction of the film layer, such as Figure 5 As shown, the X-ray diffraction pattern analysis of the heating film shows that it has a body-centered cubic structure ferrite crystal type and grows along the (110) crystal direction.
[0084] Comparative Example 3
[0085] A heating film was prepared according to the method in Example 1, wherein the material composition was consistent with that in Example 1, except that a heat treatment temperature of 500°C was selected and the temperature was kept for 60 minutes, and the other steps were the same as those in the example. Upon testing, the cross section still had columnar crystal characteristics, and the columnar crystal grain boundaries ran through the height direction of the film layer. Dry burning and wet burning tests were carried out, and the test results were as follows: Dry burning capacity: 7.5W dry burning 10 puffs resistance change = 33% (7.5W constant power on for 3s and stop for 8s dry burning in the air); Wet burning capacity: Strawberry Watermelon Ice Fruit Flavored E-liquid 7.5W puffs resistance change = 23% (7.5W puffs for 3s and stop for 15s, capacity 55mL).
[0086] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. A heating film, It is characterized in that The heating film is an iron-based alloy film, and the iron-based alloy film has an equiaxed crystal structure.
2. The heating film according to claim 1, It is characterized in that The heating film has a thickness of 0.5-3um.
3. The heating film according to claim 1, It is characterized in that The iron-based alloy film is a stainless steel film.
4. The heating film according to claim 1, It is characterized in that The iron-based alloy film comprises the following components by mass fraction: Fe: 61-72%, Cr: 16-20%, Ni: 10-15%, Mo: 2-4%; Preferably, the iron-based alloy film comprises the following components by mass fraction: Fe: 67~72%, Cr: 16-18%, Ni: 10-12%, Mo~2-3%; Preferably, the iron-based alloy film comprises the following components by mass fraction: Fe: 61~67%, Cr~18-20%, Ni~12-15%, Mo~3-4%.
5. The heating film according to claim 1, It is characterized in that The iron-based alloy film has an austenite crystal form with a face-centered cubic structure; The iron-based alloy film is measured by CuKα radiation and θ-2θ scanning, and the iron-based alloy film shows an X-ray diffraction pattern, and the X-ray diffraction peak intensity ratio of the crystal (111) plane and the (200) plane is (1-3.5):1; Preferably, the iron-based alloy film has no grain boundaries along the thickness direction.
6. The method for preparing the heat-generating film according to any one of claims 1 to 5, It is characterized in that The method comprises the following steps: step 1) preparing an iron-based alloy film by physical vapor deposition; Step 2) heat-treating the iron-based alloy film described in step 1) to form an equiaxed crystal structure, thereby obtaining the heat-generating film.
7. The method for preparing the heating film according to claim 6, It is characterized in that In the step 1), the iron-based alloy film is prepared by physical vapor deposition co-sputtering of a single metal target or physical vapor deposition sputtering of an alloy target.
8. The method for preparing the heating film according to claim 6, It is characterized in that The heat treatment method in step 2) is to heat the -2 The mixture is kept at a vacuum degree of 0.04 Pa and a temperature of 600-800°C for 30-120 min, and then cooled.
9. An atomizing core, It is characterized in that The atomizer core includes the heating film according to any one of claims 1 to 5.
10. The atomizer core according to claim 9, It is characterized in that The atomizing core comprises a heating substrate, the heating substrate is provided with the heating film, and the heating film is provided with a protective film.
11. An atomizing device, It is characterized in that The atomizing device comprises the heating film according to any one of claims 1 to 5 and / or the atomizing core according to claim 9 or 10.
Citation Information
Cited By
Heating thin film, atomization core, and atomization device