Osteochondral full-thickness repair porous composite gel scaffold material based on double-layer 3D printing and triple solution impregnation and preparation method thereof
The osteocartilage full-layer repair porous composite gel scaffold material prepared by double-layer 3D printing and triple solution impregnation technology uses the synergistic effect of biomineralization layer and ColMA layer to solve the complexity of osteocartilage defect treatment and realize the bone and efficient repair of cartilage, and biocompatible and degradable properties.
Patent Information
- Application Number
- CN202411221515.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-12-03
AI Technical Summary
The prior art has room for improvement in the treatment of osteocartilage defects, especially due to the different boundaries between cartilage and subchondral bones, tissue biochemical composition and structural mechanical properties gradients in different patients, traditional surgical sutures lack anti-infection and Promote organizational repair capabilities.
The osteocartilage full-layer repair porous composite gel scaffold material is prepared by double-layer 3D printing and triple solution impregnation technology. The lower layer is a biomineralized organic and inorganic hybrid layer. The hydroxyl group with bone-enhancing ability is formed through 3D printing and bionic mineralization technology. Apatite coating, the upper layer uses ColMA raw materials to prepare porous scaffolds and introduces factors that promote cartilage differentiation and growth of cartilage to achieve coordinated repair of the upper and lower layers.
The comprehensive repair of osteocartilage defects has been achieved. Through the synergy of the bilayer structure, efficient regeneration and repair of bone and cartilage has been promoted. The material has biocompatible, degradable and customized characteristics to meet the needs of different patients.
Smart Images

Figure CN119055840A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a preparation technology of a cartilage repair material, and in particular to a porous composite gel scaffold material for full-layer repair of osteochondrium based on double-layer 3D printing and triple solution impregnation and a preparation method thereof. Background Art
[0002] Articular osteochondral defects are an extremely common orthopedic clinical disease and an important cause of osteoarthritis and joint disability in the elderly. The prevalence of osteoarthritis alone accounts for about 10% to 12% of the global population, and for the elderly population aged >65 years, the incidence of osteoarthritis is as high as about 50%. my country has entered an aging period in 2000. After more than 20 years of development, the proportion of the elderly has increased significantly, and the degree of population aging has continued to deepen. Therefore, the repair of articular osteochondral is a clinical problem that needs to be overcome urgently.
[0003] As an efficient repair strategy, bone tissue engineering technology has shown great application prospects in the fields of bone repair and cartilage repair. Osteochondral injury generally involves damage to cartilage and subchondral bone. Its structure is more complex than that of a single bone or cartilage, and it is more difficult to treat. In recent years, some tissue engineering scaffold materials with a double-layer structure have been developed and applied to the treatment of osteochondral defects. However, due to the different boundaries between cartilage and subchondral bone in different patients, and the gradient of the biochemical composition, structure and mechanical properties of osteochondral tissue, the treatment effect still has a lot of room for improvement.
[0004] In view of the above problems, the present invention combines double-layer 3D printing and triple solution impregnation technology to prepare a double-layer heterogeneous structure of osteochondral full-layer repair porous composite gel scaffold material. The lower layer is a biomineralized organic-inorganic hybrid layer, which can efficiently promote osteogenesis; the upper layer is a porous scaffold prepared from low-concentration ColMA raw materials derived from cartilage matrix, which can induce chondrogenic differentiation in a direction. The upper and lower layers work together to achieve comprehensive repair of osteochondral defects. Summary of the invention
[0005] The purpose of the present invention is to provide a porous composite gel scaffold material for full-layer repair of osteochondral cartilage based on double-layer 3D printing and triple solution immersion and a preparation method thereof in order to address the problems that traditional surgical sutures do not have the functions of anti-infection and promoting tissue repair.
[0006] The present invention is implemented by the following technical solutions:
[0007] A method for preparing a porous composite gel scaffold material for full-layer repair of osteochondral cartilage based on double-layer 3D printing and triple solution impregnation, comprising the following steps:
[0008] 1) Using a high concentration of methacryloyl sodium alginate (AlgMA) solution for 3D printing to obtain a porous lower scaffold; the pore size of the lower scaffold is 300-500 microns;
[0009] 2) 3D printing a porous upper scaffold based on the lower scaffold using methacrylylated type I collagen (ColMA) solution; the pore size of the upper scaffold is 150-250 μm;
[0010] 3) immersing the lower scaffold in a biomimetic mineralization solution to perform a first in-situ solution immersion mineralization to form a hydroxyapatite (HA) coating with osteogenic ability on the surface of AlgMA;
[0011] 4) placing the lower scaffold in a solution of osteogenic differentiation growth factors for a second immersion, thereby introducing osteogenic differentiation growth factors into the lower scaffold;
[0012] 5) The upper scaffold is subjected to a third inversion immersion, and the upper scaffold is placed in a solution of cartilage differentiation-promoting growth factors, and after low-temperature drying and irradiation sterilization, a porous composite gel scaffold material for full-layer repair of osteochondrocytes based on double-layer 3D printing and triple solution immersion is obtained.
[0013] Furthermore, the high concentration AlgMA solution in step 1) contains a photoinitiator, wherein the AlgMA has a substitution degree of 60-90% and a concentration of 7.5-15wt%, the photoinitiator is one of LAP, Irgacure, and photoinitiator 2959, and the concentration is 0.15-0.3wt%, and the solvent is PBS;
[0014] During the 3D printing process, the conditions are to avoid light, the nozzle aperture is 200-400 microns, the printing speed is 25-35mm / s, the printing accuracy in the XY axis direction is 0.01-0.015mm, the accuracy in the Z axis direction is 0.003-0.005mm, the printing temperature is 30-35℃, the UV wavelength is 405nm, the power is 20-40W, and the curing time is 5-10min.
[0015] Furthermore, the ColMA solution in step 2) contains a photoinitiator, the degree of substitution of ColMA is 60-90%, the concentration is 4-7.5wt%, the photoinitiator is one of LAP, Irgacure, and photoinitiator 2959, the concentration is 0.15-0.3wt%, and the solvent is PBS;
[0016] During the 3D printing process, the conditions are to avoid light, the nozzle aperture is 200-400 microns, the printing speed is 20-25mm / s, the printing accuracy in the XY axis direction is 0.005-0.01mm, the accuracy in the Z axis direction is 0.002-0.004mm, the printing temperature is 30-35℃, the UV wavelength is 405nm, the power is 20-40W, and the curing time is 5-10min.
[0017] Furthermore, the formula of the biomimetic mineralization solution in step 3) is: sodium chloride 70-100mM, potassium chloride 30-50mM, magnesium sulfate 0.4-0.75mM, magnesium chloride 0.8-1.2mM, calcium chloride 4-6mM, sodium bicarbonate 0.2-0.4mM, calcium dihydrogen phosphate 1.2-1.6mM, dicalcium hydrogen phosphate 0.4-0.6mM, sodium sulfate 0.025-0.05mM, HEPES 15-22mM, and the solvent is deionized water.
[0018] Furthermore, the first in-situ solution immersion mineralization is to immerse only the lower support in the biomimetic mineralization solution under sealed conditions, with magnetic stirring at 20-40 r / min, mineralization temperature at 35-40° C., and mineralization time of 3-5 days.
[0019] Furthermore, in step 4), the osteogenic differentiation growth factor is one or more of BMP-2, KGN, TGF-β, FGF-2, FGF-9 and IGF-1, and the solution concentration is 160-220 μM;
[0020] During the impregnation process, the impregnation temperature is 4-10°C, the impregnation time is 30-60min, nitrogen is used to assist drying, the nitrogen flow rate is 1-2m / s, and the time is 20-40min.
[0021] Furthermore, in step 5), the growth factor promoting cartilage differentiation is one or more of GDF-5, bFGF, FGF-10, Afgf and EGF, and the solution concentration is 160-220 μM;
[0022] The third reversal immersion is to reverse the sample obtained in step 4) and immerse only the upper scaffold in the cartilage differentiation growth factor solution, the immersion temperature is 4-10°C, and the immersion time is 30-60min; low-temperature drying adopts nitrogen-assisted drying, the nitrogen flow rate is 1-2m / s, and the time is 20-40min.
[0023] A porous composite gel scaffold material for full-layer repair of osteochondral cartilage based on double-layer 3D printing and triple solution impregnation is obtained by any of the preparation methods described above.
[0024] Compared with the prior art, the present invention has the following advantages:
[0025] 1) The present invention uses AlgMA, ColMA, biomimetic mineralization solution, osteogenic growth factor and cartilage-promoting growth factor as raw materials, and combines 3D printing, biomimetic mineralization, triple solution impregnation and other combined processes to prepare a porous composite gel scaffold material for full-layer repair of osteochondral cartilage based on double-layer 3D printing and triple solution impregnation technology. The above raw material selection and process combination are original to the present invention.
[0026] 2) The porous composite gel scaffold material for full-thickness repair of bone cartilage in the present invention has a double-layer composite structure, which is specifically manifested as follows: macroscopically, the lower layer is a porous scaffold material with a pore size of 300-500 obtained by 3D printing using AlgMA as the raw material, and a biomineralized HA coating is applied on its surface, so that its biochemical structure and mechanical properties are compatible with the subchondral bone; at the same time, the lower layer is impregnated with osteogenic growth factors, which achieve fusion with the lower scaffold at the microscopic molecular level. The upper layer is a porous scaffold material with a pore size of 150-250 microns obtained by 3D printing using ColMA as the raw material. Collagen is an important component of the cartilage matrix. The upper scaffold printed using ColMA is impregnated with cartilage growth factors, which can simulate the physical and chemical microenvironment of the cartilage and effectively promote the regeneration and repair of the upper cartilage.
[0027] 3) The present invention realizes new applications of old processes such as 3D printing, biomimetic mineralization and solution impregnation: In combination with the structural design characteristics of the porous composite gel scaffold material for full-layer repair of osteochondrocytes in the present invention and the technical requirements in the preparation process, the present invention innovatively combines 3D printing, biomimetic mineralization and solution impregnation and other combined processes at the same time. First, a porous gel composite scaffold with upper and lower layer structures and different raw materials is prepared by double-layer continuous 3D printing technology, and the thickness of the upper and lower layers can be precisely controlled by designing a 3D printing program; then, HA coating and osteogenic growth factor are introduced into the lower scaffold in combination with triple solution impregnation and biomimetic mineralization technology, and osteogenic growth factor is introduced into the upper scaffold in turn, and strict control of the upper and lower layer boundaries can be achieved by controlling the height of the impregnation liquid level, so that the lower layer forms a composite scaffold with high modulus and osteogenic function, and the upper layer forms a composite scaffold highly similar to the natural cartilage matrix. Due to the organic synergy between the preparation processes, the upper and lower layer structures are perfectly presented, thereby achieving the purpose of efficient treatment of osteochondral defects.
[0028] 4) The porous composite gel scaffold material for full-layer repair of osteochondrocytes based on double-layer 3D printing and triple solution impregnation technology in the present invention has the functions of promoting cell ingrowth, promoting efficient and spatial repair of osteochondrocytes, and being biodegradable. By limiting the pore size of the upper and lower porous scaffold materials, adapted pore sizes are introduced for the upper and lower scaffolds respectively. The lower layer has a pore size of 300-500 microns, which conforms to the structural characteristics of trabecular bone and can promote bone ingrowth; the upper layer has a pore size of 150-250 microns, which can better promote the adhesion and proliferation of chondrocytes. The scaffold material has two different structures, the lower layer directly adsorbed in the scaffold matrix, and the osteogenic growth factor can promote the early osteogenic differentiation of cells by direct release, while the HA coating can promote osteogenesis by long-term degradation and slowly releasing calcium ions and phosphate ions in the late stage of osteogenesis; and the upper scaffold creates a physical and chemical microenvironment similar to the natural cartilage matrix through the synergistic effect of ColMA matrix and cartilage growth factor, so as to promote cartilage regeneration and repair. Furthermore, the raw materials used in the present invention are all biocompatible and degradable in vivo, and can be naturally degraded in the later stage without the need for a second operation.
[0029] 5) In the present invention, MRI, CT and other technologies can be combined to comprehensively judge the patient's osteochondral defect, and the thickness of the upper and lower layer structures of the porous composite gel scaffold material for full-layer osteochondral repair and the scale line of triple solution immersion can be jointly determined through the design of drawings before 3D printing, so as to obtain a double-layer scaffold material suitable for each patient. This technology is customizable and can meet the different needs of different patients. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 It is a schematic diagram of the preparation process of the porous composite gel scaffold material for full-layer repair of osteochondral cartilage based on double-layer 3D printing and triple solution impregnation of the present invention;
[0031] Figure 2 These are photos of the repair effect of a porous composite gel scaffold material for full-layer repair of bone cartilage based on double-layer 3D printing and triple solution immersion according to an embodiment of the present invention (a corresponds to Example 1, b corresponds to Example 3). DETAILED DESCRIPTION
[0032] The technical solution of the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments.
[0033] Comparative Example 1:
[0034] 1) A porous scaffold with a pore size of 500 μm was obtained by 3D printing (light-proof condition, nozzle aperture 200 μm, printing speed 25 mm / s, XY axis printing accuracy 0.015 mm, Z axis accuracy 0.005 mm, printing temperature 35°C, UV wavelength 405 nm, power 30 W, curing time 10 min) using a high concentration of AlgMA (60% substitution, concentration 15 wt%) / LAP photoinitiator (0.3 wt%) PBS solution;
[0035] 3) The porous scaffold was immersed in a biomimetic mineralization solution (100 mM sodium chloride, 30 mM potassium chloride, 0.4 mM magnesium sulfate, 0.8 mM magnesium chloride, 5 mM calcium chloride, 0.3 mM sodium bicarbonate, 1.3 mM calcium dihydrogen phosphate, 0.4 mM dicalcium phosphate, 0.05 mM sodium sulfate, 17 mM HEPES, and the solvent was deionized water) for the first in-situ solution immersion mineralization (mineralization conditions were sealed conditions, magnetic stirring was 20 r / min, mineralization temperature was 37°C, and mineralization time was 5 days) to form a HA coating with osteogenic ability on the surface of AlgMA;
[0036] 4) The porous scaffold is then placed just below the liquid level of a 180 μM osteogenic differentiation growth factor BMP-2 solution and fixed with a clamp for a second immersion (immersion temperature is 4°C, immersion time is 30 min), osteogenic differentiation growth factor is introduced into the lower scaffold, and nitrogen-assisted drying is performed with a nitrogen flow rate of 2 m / s for 20 min; after irradiation sterilization, a single-layer porous composite gel scaffold material is obtained.
[0037] The extract of the above materials was co-cultured with bone marrow mesenchymal stem cells (BMSCs) for 7 days, and the CCK-8 results showed that the cell survival rate was about 90.7%; it was implanted into a rabbit articular osteochondral defect model, and samples were taken after 8 weeks. New bone was generated in the joint defect area. Combined with the CT results, it was further proved that bone repair was achieved in the defect area, and no cartilage formation was observed.
[0038] Embodiment 1:
[0039] 1) Using a high concentration of AlgMA (60% substitution, concentration 15wt%) / LAP photoinitiator (0.3wt%) PBS solution for 3D printing (light-proof conditions, nozzle aperture 200 microns, printing speed 25mm / s, XY axis printing accuracy 0.015mm, Z axis accuracy 0.005mm, printing temperature 35°C, UV wavelength 405nm, power 30W, curing time 10min) to obtain a lower scaffold with an aperture of 500 microns;
[0040] 2) On the basis of the lower scaffold, a PBS solution of ColMA (60% substitution, concentration 7.5wt%) / LAP photoinitiator (0.2wt%) was continuously used for 3D printing (nozzle aperture 400 μm, printing speed 25 mm / s, XY axis printing accuracy 0.01 mm, Z axis accuracy 0.004 mm, printing temperature 35°C, UV wavelength 405 nm, power 20 W, curing time 7 min) to obtain an upper scaffold with a pore size of 250 μm;
[0041] 3) Immersing the lower scaffold in a biomimetic mineralization solution (100 mM sodium chloride, 30 mM potassium chloride, 0.4 mM magnesium sulfate, 0.8 mM magnesium chloride, 5 mM calcium chloride, 0.3 mM sodium bicarbonate, 1.3 mM calcium dihydrogen phosphate, 0.4 mM dicalcium phosphate, 0.05 mM sodium sulfate, 17 mM HEPES, and the solvent is deionized water) for the first in-situ solution immersion mineralization (mineralization conditions are sealed conditions, magnetic stirring 20 r / min, mineralization temperature 37°C, and mineralization time is 5 days) to form an HA coating with osteogenic ability on the surface of AlgMA;
[0042] 4) The lower scaffold was placed just below the liquid level of a 180 μM osteogenic differentiation growth factor BMP-2 solution and fixed with a clamp for a second immersion (immersion temperature was 4° C., immersion time was 30 min), osteogenic differentiation growth factor was introduced into the lower scaffold, and nitrogen was used for drying with a nitrogen flow rate of 2 m / s for 20 min;
[0043] 5) The upper scaffold was subjected to a third inversion immersion, keeping the upper part just below the liquid level of the 180 μM cartilage differentiation growth factor GDF-5 solution, and low-temperature drying (nitrogen-assisted drying, nitrogen flow rate 2 m / s, time 20 min) and irradiation sterilization to obtain a porous composite gel scaffold material for full-layer repair of osteochondrocytes based on double-layer 3D printing and triple solution immersion.
[0044] Compared with comparative example 1, in this embodiment, the AlgMA porous scaffold is used as the lower layer, and the upper layer ColMA porous scaffold is introduced to form a porous composite gel scaffold for full-layer repair of osteochondral. The above material extract was co-cultured with BMSCs for 7 days, and the CCK-8 results showed that the cell survival rate was about 93.7%; it was implanted into a rabbit joint osteochondral defect model, and samples were taken after 8 weeks. Hyaline cartilage was generated on the surface of the joint defect area. Combined with the CT results, it can be found that new bone is generated in the subchondral bone, indicating that the material has a good repair effect on osteochondral defects. Figure 2 Middle a.
[0045] Embodiment 2:
[0046] 1) Using a high concentration of AlgMA (60% substitution, concentration 15wt%) / LAP photoinitiator (0.3wt%) PBS solution for 3D printing (light-proof conditions, nozzle aperture 200 microns, printing speed 25mm / s, XY axis printing accuracy 0.015mm, Z axis accuracy 0.005mm, printing temperature 35°C, UV wavelength 405nm, power 30W, curing time 10min) to obtain a lower scaffold with an aperture of 500 microns;
[0047] 2) On the basis of the lower scaffold, a PBS solution of ColMA (60% substitution, concentration 7.5wt%) / LAP photoinitiator (0.2wt%) was continuously used for 3D printing (nozzle aperture 400 μm, printing speed 25 mm / s, XY axis printing accuracy 0.01 mm, Z axis accuracy 0.004 mm, printing temperature 35°C, UV wavelength 405 nm, power 20 W, curing time 7 min) to obtain an upper scaffold with a pore size of 250 μm;
[0048] 3) Immersing the lower scaffold in a biomimetic mineralization solution (100 mM sodium chloride, 30 mM potassium chloride, 0.4 mM magnesium sulfate, 0.8 mM magnesium chloride, 5 mM calcium chloride, 0.3 mM sodium bicarbonate, 1.3 mM calcium dihydrogen phosphate, 0.4 mM dicalcium phosphate, 0.05 mM sodium sulfate, 17 mM HEPES, and the solvent is deionized water) for the first in-situ solution immersion mineralization (mineralization conditions are sealed conditions, magnetic stirring 20 r / min, mineralization temperature 37°C, and mineralization time is 5 days) to form an HA coating with osteogenic ability on the surface of AlgMA;
[0049] 4) The lower scaffold was placed just below the liquid level of the 180 μM osteogenic differentiation growth factor BMP-2 solution and fixed with a clamp for a second immersion (immersion temperature was 4°C and immersion time was 30 min). The osteogenic differentiation growth factor was introduced into the lower scaffold and dried with nitrogen at a nitrogen flow rate of 2 m / s for 20 min. After irradiation sterilization, a porous composite gel scaffold material for full-layer repair of osteochondral was obtained.
[0050] Compared with Example 1, this example does not perform the third immersion in the ColMA upper porous scaffold to introduce cartilage differentiation growth factors. The extract of the above material was co-cultured with BMSCs for 7 days, and the CCK-8 results showed that the cell survival rate was about 88.1%; it was implanted into a rabbit joint osteochondral defect model, and samples were taken after 8 weeks. Turbid fibrocartilage was generated on the surface of the joint defect area, and combined with CT results, new bone was generated in the subchondral bone, indicating that the material was not effective in cartilage repair.
[0051] Embodiment 3:
[0052] 1) Using a high concentration of AlgMA (60% substitution, concentration 15wt%) / LAP photoinitiator (0.3wt%) PBS solution for 3D printing (light-proof conditions, nozzle aperture 200 microns, printing speed 25mm / s, XY axis printing accuracy 0.015mm, Z axis accuracy 0.005mm, printing temperature 35°C, UV wavelength 405nm, power 30W, curing time 10min) to obtain a lower scaffold with an aperture of 500 microns;
[0053] 2) On the basis of the lower scaffold, a PBS solution of ColMA (60% substitution, concentration 7.5wt%) / LAP photoinitiator (0.2wt%) was continuously used for 3D printing (nozzle aperture 400 μm, printing speed 25 mm / s, XY axis printing accuracy 0.01 mm, Z axis accuracy 0.004 mm, printing temperature 35°C, UV wavelength 405 nm, power 20 W, curing time 7 min) to obtain an upper scaffold with a pore size of 250 μm;
[0054] 3) The upper scaffold is immersed in the solution, keeping the upper part just below the liquid level of the chondrogenic growth factor GDF-5 solution with a concentration of 180 μM, and low-temperature drying (nitrogen-assisted drying, nitrogen flow rate 2 m / s, time 20 min) and irradiation sterilization to obtain a porous composite gel scaffold material for osteochondrocyte repair.
[0055] Compared with Example 1, this embodiment reduces the steps of impregnating the AlgMA lower scaffold to form a HA coating and adsorbing osteogenic differentiation growth factors. The above material extract was co-cultured with BMSCs for 7 days. The CCK-8 results showed that the cell survival rate was about 85.6%. It was implanted into a rabbit joint osteochondral defect model. After 8 weeks, the joint defect area showed poor repair effect. Combined with the CT results, it was further proved that only a small amount of new bone was generated in the subchondral bone. Overall, the material showed poor repair effect for osteochondral defects. Figure 2 Middle b.
Claims
1. A method for preparing a porous composite gel scaffold material for full-layer repair of osteochondral cartilage based on double-layer 3D printing and triple solution impregnation, characterized in that: The following steps are involved: 1) Using a high concentration of methacryloyl sodium alginate (AlgMA) solution for 3D printing to obtain a porous lower scaffold; The pore size of the lower support is 300-500 μm; 2) 3D printing a porous upper scaffold on the lower scaffold using methacryloyl type I collagen (ColMA) solution; The pore size of the upper support is 150-250 μm; 3) immersing the lower support in a biomimetic mineralization solution to perform a first in-situ solution immersion mineralization; 4) placing the lower scaffold in a solution of osteogenic differentiation growth factors for a second immersion; 5) The upper scaffold is subjected to a third inversion immersion, and the upper scaffold is placed in a solution of cartilage differentiation-promoting growth factors, and after low-temperature drying and irradiation sterilization, a porous composite gel scaffold material for full-layer repair of osteochondrocytes based on double-layer 3D printing and triple solution immersion is obtained.
2. The method for preparing a porous composite gel scaffold material for full-layer repair of osteochondrocytes based on double-layer 3D printing and triple solution impregnation according to claim 1, characterized in that: The high concentration AlgMA solution in step 1) contains a photoinitiator, wherein the AlgMA has a substitution degree of 60-90% and a concentration of 7.5-15wt%, the photoinitiator is one of LAP, Irgacure, and photoinitiator 2959, and the concentration is 0.15-0.3wt%, and the solvent is PBS; The 3D printing parameters are: light-proof conditions, nozzle aperture 200-400 microns, printing speed 25-35mm / s, printing accuracy in the XY axis direction 0.01-0.015mm, Z axis direction accuracy 0.003-0.005mm, printing temperature 30-35℃, UV wavelength 405nm, power 20-40W, and curing time 5-10min.
3. The method for preparing a porous composite gel scaffold material for full-layer repair of osteochondrocytes based on double-layer 3D printing and triple solution impregnation according to claim 1, characterized in that: The ColMA solution in step 2) contains a photoinitiator, the substitution degree of ColMA is 60-90%, the concentration is 4-7.5wt%, the photoinitiator is one of LAP, Irgacure, and photoinitiator 2959, the concentration is 0.15-0.3wt%, and the solvent is PBS; The 3D printing parameters are: light-proof conditions, nozzle aperture 200-400 microns, printing speed 20-25mm / s, printing accuracy in the XY axis direction 0.005-0.01mm, accuracy in the Z axis direction 0.002-0.004mm, printing temperature 30-35℃, UV wavelength 405nm, power 20-40W, and curing time 5-10min.
4. The method for preparing a porous composite gel scaffold material for full-layer repair of osteochondrocytes based on double-layer 3D printing and triple solution impregnation according to claim 1, characterized in that: The formula of the biomimetic mineralization solution in step 3) is: sodium chloride 70-100mM, potassium chloride 30-50mM, magnesium sulfate 0.4-0.75mM, magnesium chloride 0.8-1.2mM, calcium chloride 4-6mM, sodium bicarbonate 0.2-0.4mM, calcium dihydrogen phosphate 1.2-1.6mM, dicalcium hydrogen phosphate 0.4-0.6mM, sodium sulfate 0.025-0.05mM, HEPES 15-22mM, and the solvent is deionized water.
5. The method for preparing a porous composite gel scaffold material for full-layer repair of osteochondrocytes based on double-layer 3D printing and triple solution impregnation according to claim 1, characterized in that: The first in-situ solution immersion mineralization is to immerse only the lower support in the bionic mineralization solution under sealed conditions, with magnetic stirring at 20-40 r / min, mineralization temperature at 35-40° C., and mineralization time of 3-5 days.
6. The method for preparing a porous composite gel scaffold material for full-layer repair of osteochondrocytes based on double-layer 3D printing and triple solution impregnation according to claim 1, characterized in that: Step 4) the osteogenic differentiation growth factor in the osteogenic differentiation growth factor solution is one or more of BMP-2, KGN, TGF-β, FGF-2, FGF-9 and IGF-1, and the concentration is 160-220 μM; During the second impregnation process, the impregnation temperature is 4-10°C, the impregnation time is 30-60min, and nitrogen-assisted drying is adopted after the impregnation is completed, with a nitrogen flow rate of 1-2m / s and a time of 20-40min.
7. The method for preparing a porous composite gel scaffold material for full-layer repair of osteochondrocytes based on double-layer 3D printing and triple solution impregnation according to claim 1, characterized in that: Step 5) the cartilage differentiation growth factor in the cartilage differentiation growth factor solution is one or more of GDF-5, bFGF, FGF-10, Afgf and EGF, and the concentration is 160-220 μM; The third reversal immersion is to reverse the sample obtained in step 4) and immerse only the upper scaffold in the cartilage differentiation growth factor solution, the immersion temperature is 4-10°C, and the immersion time is 30-60min; low-temperature drying adopts nitrogen-assisted drying, the nitrogen flow rate is 1-2m / s, and the time is 20-40min.
8. A porous composite gel scaffold material for full-layer repair of osteochondral cartilage based on double-layer 3D printing and triple solution impregnation, characterized in that: The method is adopted as described in any one of claims 1 to 7.