Preparation method of carbon nitride / clay / biochar amphiphilic aerogel and application of carbon nitride / clay / biochar amphiphilic aerogel in oil-water separation

By using vapor deposition method in hot air, carbon nitride/clay/biochar amphiphilic aerogels are prepared, the problem of biochar aerogel not meeting the performance standards in large-area oil leakage treatment is solved, and efficient adsorption and Recyclable capacity simplifies the preparation process and improves the stability and application value of the material.

CN119056404APending Publication Date: 2024-12-03XINJIANG UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310638377.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-06-01
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

When existing biochar aerogels treat large-area oil leakage, the skeleton collapses due to stacking between carbon layers, and their performance does not meet the standards. The traditional preparation methods are harsh, making it difficult to achieve efficient adsorption and recycling.

Method used

The preparation method of carbon nitride/clay/biochar amphiphilic aerogel is adopted to create a less oxygen atmosphere in hot air through vapor deposition. The carbon nitride is firmly loaded on clay/biochar through chemical bonds to enhance carbon gas The stability and specific surface area of ​​the gel are used to improve its hydrophilic properties and adsorption capacity by combining clay and biomass cellulose.

Benefits of technology

It realizes the efficient adsorption and recovery capability of carbon nitride/clay/biochar amphiphilic aerogel, which is suitable for large-area oil leakage treatment, simplifies the preparation process, and improves the stability and application value of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention belongs to the technical field of biochar aerogel preparation, and provides a preparation method of carbon nitride / clay / biochar amphiphilic aerogel. According to the method, biomass cellulose is taken as a raw material, clay is taken as a reinforcing agent, an oxygen-deficient atmosphere is created in hot air through a vapor deposition method in a muffle furnace, and the carbon nitride / clay / charcoal amphiphilic aerogel is obtained. According to the invention, a low-oxygen atmosphere is created in hot air through a vapor deposition method to replace a traditional inert atmosphere condition for preparing biochar. According to the preparation method, firm deposition of carbon nitride is realized through chemical bonding and intermolecular synergistic effect, and the carbon nitride is uniform in dispersity, so that the stability and the specific surface area of the carbon aerogel are increased, and the recoverability and the adsorption capacity of the carbon aerogel are improved. The carbon nitride / clay / biochar amphiphilic aerogel has super-hydrophilicity and super-lipophilicity, has good adsorption capacity and recoverability on floating oil, can be used for large-area oil leakage treatment, and has practical application value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of environmental protection, and specifically relates to a preparation method of carbon nitride / clay / biochar amphiphilic aerogel and application thereof in oil-water separation. Background Art

[0002] In today's society, humans, animals and plants are facing potential health and safety risks caused by oily wastewater. Activated carbon has a highly developed internal void structure and a high specific surface area, and has a high adsorption capacity for various oils and organic solvents. However, it does not have the ability to recover when dealing with large-scale oil spills, making it difficult to achieve a reversible process of adsorption-desorption, which can easily cause secondary pollution. Biochar aerogel has the advantages of high specific surface area, low density and easy recycling of gel, as well as the high adsorption characteristics of activated carbon, and is widely used in the treatment of oily wastewater. However, due to the strong intermolecular forces between the carbon layers, the sheets are stacked during the self-assembly process, causing the skeleton of the carbon gel to collapse, so that its performance often does not reach the theoretical value. This problem greatly limits its practical application. Clay minerals have a special structure and morphology, and have the characteristics of good dispersibility, high specific surface area, good mechanical properties, abundant reserves, and low cost. They are excellent natural adsorbents. When clay meets water, its volume can expand to several times its original volume and is highly dispersed in water. The highly swollen and dispersed clay slurry is compounded into the carbon gel, and the highly dispersed clay enters between the carbon layers, which can effectively alleviate the stacking effect between the carbon layers and enhance the skeleton structure of the carbon gel. Chinese patent document CN 110540187 discloses a method for preparing a clay / carbon aerogel material, which is to mechanically homogenize waste textiles of natural cellulose such as cotton, linen, silk, and wool, and then sol-gel and carbonize them with clay particles to obtain an aerogel with adsorption effect. Although the aerogel material effectively alleviates the stacking effect between the carbon layers and enhances the skeleton structure of the carbon gel to a certain extent. However, there are still problems such as the carbonization conditions require inert atmosphere conditions and harsh preparation conditions, which limit its practical application.

[0003] In view of this, the present invention proposes a method for preparing a carbon nitride / clay / biochar amphiphilic aerogel, which uses biomass cellulose as raw material and clay as a reinforcing agent, and creates a low-oxygen atmosphere in the air through a carbon nitride vapor deposition method to obtain a carbon nitride / clay / biochar amphiphilic aerogel. Through this grafting process, carbon nitride is firmly loaded on clay / biochar through chemical bonding, which increases the stability and specific surface area of ​​the carbon aerogel on the one hand; on the other hand, carbon nitride has strong hydrophilicity, and the dispersibility of carbon nitride can be increased by loading, thereby improving the hydrophilicity of the composite material. In addition, the carbon nitride / clay / biochar amphiphilic aerogel has both the unique structure of aerogel and the excellent adsorption performance of carbon materials, and has a stable skeleton structure, which is easy to separate and recycle, providing a new idea for the development of new biochar composite materials, and is conducive to the efficient utilization of natural biomass. The preparation method of the carbon nitride / clay / biochar amphiphilic aerogel of the present invention creates a low-oxygen atmosphere in hot air by a vapor deposition method to replace the inert atmosphere conditions for traditional preparation of biochar. The preparation method is simple, and the gel has good adsorption and recovery capabilities for floating oil, can be used for large-scale oil spill treatment, and has practical application value. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing carbon nitride / clay / biochar amphiphilic aerogel by creating a low-oxygen atmosphere in hot air through a gas phase deposition method to replace the inert atmosphere conditions for traditional preparation of biochar; to firmly deposit carbon nitride on clay / biochar through chemical bonding, thereby increasing the stability and specific surface area of ​​the carbon aerogel, improving its recyclability and adsorption capacity, and using it for rapid separation of oil-water mixtures; and to provide new ideas for the development of new biochar composite materials through the combination of clay and biomass cellulose, thereby realizing the resource utilization of natural biomass.

[0005] The idea of ​​the present invention is to introduce clay into cellulose and PVA as the skeleton structure and physical cross-linking sites, physically cross-link the clay through hydrogen bonds, and use glutaraldehyde as a chemical cross-linking agent to chemically cross-link to prepare clay / cellulose composite aerogel, and create a low-oxygen atmosphere through vapor deposition method to replace the traditional inert conditions to prepare carbon nitride / clay / biochar amphiphilic aerogel, and use it for the rapid separation of oil-water mixtures.

[0006] The first aspect of the present invention provides: creating a low-oxygen atmosphere in hot air by a vapor deposition method to replace the inert atmosphere conditions for traditional preparation of biochar.

[0007] The second aspect of the present invention provides: a method for preparing the above-mentioned carbon nitride / clay / biochar amphiphilic aerogel, which specifically has the following characteristics, comprising the following steps: Step 1, preparation of clay / cellulose xerogel: after mixing and stirring the biomass source cellulose slurry, PVA solution and clay slurry for 1 hour, adjust the pH and add glutaraldehyde, continue to stir the obtained mixture for 1 hour, and then obtain the clay / cellulose xerogel through ultrasonic defoaming, heat curing and freeze drying.

[0008] Step 2, preparation of carbon nitride / clay / biochar amphiphilic aerogel: add melamine into a small crucible, seal it with aluminum foil, pierce holes into it and put it into a large crucible, place the clay / cellulose dry gel on the surface of the aluminum foil, seal it with aluminum foil, and finally place it in a muffle furnace for high-temperature calcination.

[0009] In one embodiment, in the first step, the extraction method of biomass-derived cellulose is as follows: firstly, the biomass powder is placed in an acidic aqueous solution, heated and stirred, centrifuged and washed with water to obtain a pretreated cellulose homogenate; then the pretreated cellulose homogenate is placed in a NaOH solution, stirred at room temperature, centrifuged, stirred under distilled water at room temperature, and centrifuged to obtain a biomass-derived cellulose homogenate. Wherein, the ratio of biomass powder to acidic aqueous solution is 1:10 to 1:60; the pH of the acidic aqueous solution is 1 to 3; the heating temperature is 60 to 90°C; the heating temperature is 100 to 15 ... o C; heating and stirring for 3-8 h; biomass powder: NaOH solution / distilled water = 1:20-1:100; stirring at room temperature for 3-8 h.

[0010] In one embodiment, in the first step, the mass percentage of the biomass source cellulose homogenate is 2% to 5%; the concentration of the PVA solution is 0.03 to 0.1 g / mL; the mass percentage of the clay homogenate is 0 to 9.7 wt %; the pH range is 4 to 6; the mass percentage of glutaraldehyde is 20 to 50 wt %; the ultrasonic time is 20 to 60 min; and the curing conditions are 60 to 90 o C, 2~6 h; freeze-drying time is 14~42 h.

[0011] In one embodiment, in the second step, clay / cellulose xerogel: melamine = 1:2-1:8; the heating rate is 1-10 o C, the holding time is 2~6 h, and the calcination temperature is 500~550 o C.

[0012] In one embodiment, the biomass in step 1 includes beet pulp, cotton stalks, peanut shells, corn cobs, grapefruit peels, walnut shells, etc.

[0013] In one embodiment, the clay in step 2 includes montmorillonite, bentonite, kaolin and the like.

[0014] In one embodiment, all ratios in the method for preparing the carbon nitride / clay / biochar amphiphilic aerogel are mass ratios.

[0015] The third aspect of the present invention provides: Application of the above carbon nitride / clay / biochar amphiphilic aerogel in oil-water separation.

[0016] The present invention has the following advantages: (1) The raw materials of the prepared carbon nitride / clay / biochar amphiphilic aerogel are waste biomass materials, which can achieve the quality improvement of biomass waste. (2) The low-oxygen atmosphere is created in hot air by the vapor deposition method to replace the inert atmosphere conditions for traditional preparation of biochar. The preparation method is simple and has practical application value. (3) There is chemical bonding in the prepared carbon nitride / clay / biochar amphiphilic aerogel, the carbon nitride has good dispersion and firm loading, and the stability of the biochar gel is improved. (4) The adsorption performance of carbon nitride / clay / biochar amphiphilic aerogel on oil products provides a reference for sewage treatment and ecological environment restoration.

[0017] Description of the drawings: Figure 1 It is a digital photo of the carbon nitride / clay / biochar amphiphilic aerogel-3 and the clay / biochar aerogel in the present invention; Figure 2 This is a digital photo of the contact angle of the carbon nitride / clay / biochar amphiphilic aerogel-3 of the present invention; Figure 3 This is a comparison chart of the adsorption capacity of the carbon nitride / clay / biochar amphiphilic aerogel-3 and the clay / biochar aerogel in the present invention; Figure 4 This is a test chart of the adsorption capacity of carbon nitride / clay / biochar amphiphilic aerogel-3 of the present invention for oil and water; Figure 5 This is a test diagram of floating oil adsorption of carbon nitride / clay / biochar amphiphilic aerogel-3 in the present invention.

[0018] Specific implementation measures The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. However, it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. If specific techniques or conditions are not specified in the examples, they are carried out according to the techniques described in the literature in this area or according to the product instructions. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be obtained commercially.

[0019] Example 1: Synthesize carbon nitride / clay / biochar amphiphilic aerogel-1 according to the following steps: (1) Preparation of clay / cellulose xerogel: 8.34 g of biomass cellulose slurry, 3 mL of PVA solution (0.05 g / mL), and 3.34 g of clay slurry (9.1 wt%) were mixed and stirred for 1 h, the pH was adjusted to 5, and 0.2 g of glutaraldehyde (25 wt%) was added. The resulting mixture was stirred for 1 h, ultrasonically treated for 20 min, and then placed in 75 o C oven for curing / crosslinking treatment, and finally freeze-dried for 32 h to obtain clay / cellulose xerogel. (2) Preparation of C3N4 / clay / biochar amphiphilic aerogel-1: 1 g of melamine was added to a small crucible, sealed with aluminum foil and placed in a large crucible, and the clay / cellulose xerogel was placed on the surface of the aluminum foil, sealed with aluminum foil, and finally placed in a muffle furnace at 550 o C high temperature calcination, heating rate 5 o C / min, and the holding time is 2 h.

[0020] Example 2: Synthesize carbon nitride / clay / biochar amphiphilic aerogel-3 according to the following steps: (1) Preparation of clay / cellulose xerogel: 8.34 g of biomass cellulose slurry, 3 mL of PVA solution (0.05 g / mL), and 3.34 g of clay slurry (9.1 wt%) were mixed and stirred for 1 h, the pH was adjusted to 5, and 0.2 g of glutaraldehyde (25 wt%) was added. The resulting mixture was stirred for 1 h, ultrasonically treated for 20 min, and then placed in 75 o C oven for curing / crosslinking treatment, and finally freeze-dried for 32 h to obtain clay / cellulose xerogel. (2) Preparation of C3N4 / clay / biochar amphiphilic aerogel-3: 3 g of melamine was added to a small crucible, which was sealed with aluminum foil and pierced with holes and placed in a large crucible. The clay / cellulose xerogel was placed on the surface of the aluminum foil, which was sealed with aluminum foil, and finally placed in a muffle furnace at 550 °C. o C high temperature calcination, heating rate 5 o C / min, and the holding time is 2 h.

[0021] Figure 1 This is a digital photo of the carbon nitride / clay / biochar amphiphilic aerogel-3 and the clay / biochar aerogel in the present invention. From the photo, it can be seen that the carbon nitride is uniformly deposited in the carrier. Figure 2 This is a digital photo of the contact angle of the carbon nitride / clay / biochar amphiphilic aerogel-3 in the present invention. It can be seen that the water and oil contact angles of the sample are both 0 o , the surface of the carbon nitride / clay / biochar amphiphilic aerogel-3 in the present invention is a super hydrophilic and super oleophilic material.

[0022] Figure 3 This is a comparison chart of the adsorption capacity of the carbon nitride / clay / biochar amphiphilic aerogel-3 and the clay / biochar aerogel in the present invention. It can be seen that the deposition of carbon nitride greatly improves the adsorption amount of the clay / biochar aerogel. The adsorption amount of the carbon nitride / clay / biochar amphiphilic aerogel-3 is increased by 66% compared with the clay / biochar aerogel.

[0023] Figure 4 This is a test diagram of the adsorption capacity of the carbon nitride / clay / biochar amphiphilic aerogel-3 in the present invention for oil and water. It can be seen that the carbon nitride / clay / biochar amphiphilic aerogel-3 in the present invention has good adsorption capacity for both water and oil and is a very good adsorption material.

[0024] Figure 5 This is a test chart of the adsorption capacity of carbon nitride / clay / biochar amphiphilic aerogel-3 for floating oil in the present invention, which shows that the carbon nitride / clay / biochar amphiphilic aerogel-3 in the present invention has good floating oil adsorption and oil-water separation capabilities and can be used for large-area floating oil adsorption.

[0025] Example 3: Synthesize carbon nitride / clay / biochar amphiphilic aerogel-5 according to the following steps: (1) Preparation of clay / cellulose xerogel: 8.34 g of biomass cellulose slurry, 3 mL of PVA solution (0.05 g / mL), and 3.34 g of clay slurry (9.1 wt%) were mixed and stirred for 1 h, the pH was adjusted to 5, and 0.2 g of glutaraldehyde (25 wt%) was added. The resulting mixture was stirred for 1 h, ultrasonically treated for 20 min, and then placed in 75 o C oven for curing / crosslinking treatment, and finally freeze-dried for 32 h to obtain clay / cellulose xerogel. (2) Preparation of carbon nitride / clay / biochar amphiphilic aerogel-5: 5 g of melamine was added to a small crucible, which was sealed with aluminum foil and pierced with holes and placed in a large crucible. The clay / cellulose xerogel was placed on the surface of the aluminum foil, which was sealed with aluminum foil, and finally placed in a muffle furnace at 550 °C. o C high temperature calcination, heating rate 5 o C / min, and the holding time is 2 h.

[0026] Comparative Cases Difference from the implementation case: No carbon nitride is deposited during high temperature calcination in the third step.

[0027] (1) Preparation of clay / cellulose xerogel: 8.34 g of biomass cellulose slurry, 3 mL of PVA solution (0.05 g / mL), and 3.34 g of clay slurry (5.6 wt%) were mixed and stirred for 1 h, the pH was adjusted to 5, and 0.2 g of glutaraldehyde (25 wt%) was added. The resulting mixture was stirred for 1 h, ultrasonically treated for 20 min, and then placed in 75 o C oven for curing / crosslinking treatment, and finally freeze-dried for 32 h to obtain clay / cellulose xerogel. (2) Preparation of clay / biochar aerogel: The clay / cellulose xerogel was placed in a muffle furnace at 550 o C high temperature calcination, heating rate 5 o C / min, and the holding time is 2 h.

[0028] In the above case, the preparation steps of bio-source cellulose homogenate are as follows: 60 mL of distilled water is placed in a 100 mL high-necked beaker, 3.0 g of beet pulp powder is weighed and added to the distilled water, and then concentrated hydrochloric acid is used to adjust the pH to 1.5, and the mixture is heated at 85 o C water bath for 4 h to remove pectin, centrifuge at low speed (2000 rpm, 2 min), wash with distilled water until neutral, add 100 mL of NaOH solution (0.1 mol / L) and stir continuously for 3 h, centrifuge at low speed (2000 rpm, 2 min), add 100 mL of distilled water and stir at room temperature for 1 h. Centrifuge at low speed (2000 rpm, 2 min), wash with distilled water until neutral, and obtain beet pulp fiber homogenate for use.

Claims

1. A method for preparing carbon nitride / clay / biochar amphiphilic aerogel, characterized in that: The invented gel uses clay / biomass-derived cellulose aerogel as a carrier, and carbon nitride is uniformly and firmly loaded on the carrier by a vapor deposition method, and a low-oxygen atmosphere is created in hot air to prepare a biochar composite gel.

2. The method for preparing the carbon nitride / clay / biochar amphiphilic aerogel according to claim 1 is specifically implemented according to the following steps: Step 1, preparation of clay / cellulose xerogel: After mechanically stirring the biomass-derived cellulose slurry, PVA solution and clay slurry for 1 h, the pH was adjusted and glutaraldehyde was added. After the obtained mixture was stirred for another 1 h, the clay / cellulose xerogel was obtained by ultrasonic defoaming, heat curing and freeze drying.

3. Step 2, preparation of carbon nitride / clay / biochar amphiphilic aerogel: Add melamine into a small crucible, seal it with aluminum foil, pierce holes in it and put it into a large crucible, place the clay / cellulose dry gel obtained in step 1 on the surface of the aluminum foil, seal it with aluminum foil, and place it in a muffle furnace for high-temperature calcination.

4. The method for preparing the carbon nitride / clay / biochar amphiphilic aerogel according to claim 2, characterized in that: In the first step, the extraction step of biomass-derived cellulose is as follows: placing biomass powder in an acidic aqueous solution, heating and stirring, centrifuging and washing with water to obtain a pretreated cellulose homogenate; The pretreated cellulose homogenate was placed in a NaOH solution and stirred at room temperature, centrifuged, and then stirred in distilled water at room temperature and centrifuged to obtain a biomass-derived cellulose homogenate.

5. Among them, biomass powder: acidic aqueous solution = 1:10~1:60; the pH of the acidic aqueous solution is 1~3; the heating temperature is 60~90 o C; heating and stirring for 3-8 h; biomass powder: NaOH solution / distilled water = 1:20-1:100; stirring at room temperature for 3-8 h.

6. The method for preparing the carbon nitride / clay / biochar amphiphilic aerogel according to claim 2, characterized in that: In the first step, the mass percentage of the biomass source cellulose homogenate is 2% to 5%; the concentration of the PVA solution is 0.03 to 0.1 g / mL; the mass percentage of the clay homogenate is 0 to 9.7 wt %; the pH range is 4 to 6; the mass percentage of glutaraldehyde is 20 to 50 wt %; the ultrasonic time is 20 to 60 min; and the curing conditions are 60 to 90 o C, 2~6 h; freeze-drying time is 14~42 h.

7. In the second step, the ratio of clay / cellulose xerogel to melamine is 1:2 to 1:8; the heating rate is 1 to 10 o C, the holding time is 2~6 h, and the calcination temperature is 500~550 o C.

8. The method for preparing the carbon nitride / clay / biochar amphiphilic aerogel according to claim 2, characterized in that: All ratios in the preparation method of carbon nitride / clay / biochar amphiphilic aerogel are mass ratios.

9. The method for preparing the carbon nitride / clay / biochar amphiphilic aerogel according to claim 2, characterized in that: The biomass in the first step includes beet pulp, cotton stalks, peanut shells, corn cobs, grapefruit peels, walnut shells, etc.; the clay in the second step includes montmorillonite, bentonite and kaolin, etc.

10. Application of carbon nitride / clay / biochar amphiphilic aerogel in oil-water separation.