Magnetic porous integral adsorbent capable of simultaneously enriching triazole pesticides, Cr (III) and Cr (VI) as well as preparation method and application of magnetic porous integral adsorbent

The prepared magnetic porous integral adsorbent uses B-N coordination, hydrogen bonding and π-π stacking, which solves the problem that the prior art cannot detect triazole pesticides and different chromium forms at the same time, and achieves efficient sample enrichment and analysis , has good practical application value.

CN119056419AActive Publication Date: 2024-12-03XIAMEN UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411339540.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-12-03
Estimated Expiration
2044-09-25

AI Technical Summary

Technical Problem

The prior art cannot simultaneously and efficiently detect triazole pesticides and different forms of chromium (Cr), especially Cr(III) and Cr(VI), while triazole pesticides and different forms of chromium (Cr) are present in the environment. The concentration is low and the sample substrate is complex, and existing methods are difficult to achieve effective enrichment and analysis.

Method used

Ethylene boron anhydride pyridine soluble (VAP) and 1-allyl-3-methylimidazole bistrifluoromethanesulfonimide salt (MAT) as functional monomers, combining ethylene glycol dimethacrylate and Divinylbenzene as crosslinking agent, n-propanol and 1,4-butanediol as pore-generator, azobisisobutyronitrile as initiator, and modified Fe3O4 nanoparticles were prepared by ultrasonication into a homogeneous solution and polymerization reaction. Magnetic porous monolithic adsorbent uses B-N coordination, hydrogen bonding and π-π stacking to achieve efficient enrichment of triazole pesticides and different forms of Cr.

Benefits of technology

It realizes efficient extraction and detection of triazole pesticides and different forms of Cr. It has the advantages of simple operation, low cost, long service life, environmentally friendly and high enrichment efficiency, and is suitable for pretreatment of environmental samples.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119056419A_ABST
    Figure CN119056419A_ABST
Patent Text Reader

Abstract

The invention discloses a magnetic porous integral adsorbent capable of simultaneously enriching triazole pesticides, Cr (III) and Cr (VI) as well as a preparation method and application of the magnetic porous integral adsorbent, and relates to the field of sample pretreatment, the magnetic porous integral adsorbent is prepared by taking an ethylene boric anhydride pyridine solvate and 1-allyl-3-methylimidazole bis (trifluoromethanesulfonyl) imide salt as bifunctional monomers and utilizing an in-situ polymerization technology. The adsorbent can simultaneously enrich four triazole pesticides and two forms of Cr through multiple effects of B-N coordination, hydrogen bonds, pi-pi accumulation and the like. Meanwhile, the prepared adsorbent has the advantages of being simple and convenient to operate, low in cost, long in service life, low in organic reagent consumption, environmentally friendly, high in enrichment efficiency and the like, and therefore the prepared magnetic porous integral adsorbent has good practical application value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of sample pretreatment, and in particular to a magnetic porous monolithic adsorbent capable of simultaneously enriching triazole pesticides, Cr(III) and Cr(VI), and a preparation method and application thereof. Background Art

[0002] Triazole pesticides are widely used to control diseases of various crops, vegetables, and fruits. However, during production and application, triazole pesticides inevitably seep into aquatic ecosystems such as rivers and lakes. Studies have shown that triazole compounds, due to their potential mutagenicity and carcinogenicity, can significantly interfere with the human endocrine system. Cr (Cr) originates from various industrial wastewaters and exhaust emissions. For example, large amounts of Cr-containing wastewater are generated during production processes in industries such as leather making, smelting, and electroplating. Cr exists in the environment primarily in two forms: Cr(III) and Cr(VI). Cr(III) is an essential trace element for the human body and participates in various biological processes in the body. Cr(VI), due to its strong oxidizing and high permeability, can induce mutations and is carcinogenic. Therefore, speciation analysis of Cr is essential. Therefore, based on practical needs, there is an urgent need to develop sensitive and reliable methods for the detection of triazole pesticides and different forms of Cr in environmental samples.

[0003] At present, the commonly used determination methods for triazole pesticides are gas chromatography and high-performance liquid chromatography, and the commonly used speciation analysis methods for Cr include flame atomic absorption spectrometry, electrothermal atomic absorption spectrometry, and inductively coupled plasma mass spectrometry. There is no literature report on a method that can simultaneously enrich and detect triazole pesticides and different forms of chromium. Summary of the Invention

[0004] The purpose of the present invention is to solve the above-mentioned problems in the prior art and provide a magnetic porous monolithic adsorbent and a preparation method thereof that can simultaneously and efficiently extract triazole pesticides and different forms of chromium in environmental samples. The magnetic porous monolithic adsorbent is prepared in situ in a capillary using ethylene boron anhydride pyridine solute (VAP) and 1-allyl-3-methylimidazolium bistrifluoromethanesulfonyl imide salt (MAT) as bifunctional monomers, achieving the simultaneous and efficient enrichment of triazole pesticides and different forms of chromium for the first time.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] A method for preparing a magnetic porous monolithic adsorbent capable of simultaneously enriching triazole pesticides, Cr(III) and Cr(VI) comprises the following steps:

[0007] 1) functional monomers, cross-linking agents, porogens, initiators, and magnetic nanoparticles are mixed in proportion and ultrasonically mixed into a uniform solution;

[0008] 2) injecting the prepolymer solution mixed in step 1) into a container, sealing it, and initiating a polymerization reaction at a certain temperature;

[0009] 3) After the polymerization reaction is completed, rinse it with a certain volume of methanol or acetonitrile, and then rinse and activate it with methanol or acetonitrile before use;

[0010] The functional monomers are VAP and MAT;

[0011] The cross-linking agents are ethylene glycol dimethacrylate (EDMA) and divinylbenzene (DVB);

[0012] The porogens are n-propanol and 1,4-butanediol.

[0013] The added amount of the VAP and MAT is 10% to 30% of the total mass of the prepolymerization solution, and the mass ratio of VAP to MAT is 1:4 to 4:1.

[0014] The added amount of the EDMA and DVB is 10% to 30% of the total mass of the prepolymerization solution, and the mass ratio of the EDMA to DVB is 1:3 to 3:1.

[0015] The added amount of the n-propanol and 1,4-butanediol is 40% to 90% of the total mass of the prepolymerization solution, and the mass ratio of the n-propanol to 1,4-butanediol is 1:3 to 3:1.

[0016] The initiator is azobisisobutyronitrile (AIBN); the added amount of AIBN is 0.2-4.0 mg / 100 mg of the prepolymer solution.

[0017] The magnetic nanoparticles are modified Fe3O4 nanoparticles; the mass of the added magnetic nanoparticles is 0.5-5.0 mg / 100 mg of the prepolymer solution.

[0018] In step 2), the polymerization reaction temperature is 60 to 80° C., and the polymerization reaction time is 8 to 24 hours.

[0019] In step 3), the certain volume is 1.0 to 10 mL.

[0020] The adsorbent prepared by the present invention can simultaneously enrich four triazole pesticides and two forms of Cr through multiple effects such as BN coordination, hydrogen bonding and π-π stacking.

[0021] Because the concentration of pollutants in the environment is very low and the actual sample substrate is relatively complex, the present invention performs a pretreatment to enrich the sample, utilizes a chelating agent to react with Cr to generate a complex with ultraviolet absorption, and then uses a high-performance liquid chromatography coupled with an ultraviolet detector for determination. By optimizing the chromatographic method, the simultaneous determination of triazole pesticides and different forms of Cr can be achieved.

[0022] Specifically, the sample containing triazole pesticides, Cr(III) and Cr(VI) is subjected to adsorption pre-treatment by the magnetic porous monolithic adsorbent, followed by desorption, and finally the triazole pesticides and different forms of Cr are simultaneously analyzed by a chromatographic detection method.

[0023] In the present invention, a complexing agent is used to convert Cr(III) and Cr(VI) into metal-organic complexes that can be detected by HPLC-DAD during pre-adsorption treatment; ultrapure water and acetonitrile are used as mobile phases, and a gradient elution program is set: 0-11.0 min, 53% acetonitrile; 11.0-15.0 min, 53%-70% acetonitrile; 15.0-18.0 min, 70% acetonitrile; 18.0-22.0 min, 70%-53% acetonitrile; 22.0-25.0 min, 53% acetonitrile, thereby achieving simultaneous detection of triazole pesticides and different forms of Cr.

[0024] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:

[0025] This invention synthesizes, for the first time, a magnetic porous monolithic adsorbent capable of simultaneously and efficiently extracting triazole pesticides and various forms of chromium. Because the adsorbent is rich in boron, nitrogen, and aromatic functional groups, it achieves efficient and simultaneous extraction of triazole pesticides and chromium complexes through BN coordination, hydrogen bonding, and π-π stacking. Furthermore, the prepared adsorbent offers advantages such as simple operation, low cost, long service life, low organic reagent consumption, environmental friendliness, and high enrichment efficiency. Therefore, the magnetic porous monolithic adsorbent prepared by this invention has excellent practical application value. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 Schematic diagram of the synthesis reaction of the magnetic porous monolithic adsorbent in Example 2.

[0027] Figure 2 This is the infrared spectrum of the magnetic porous monolithic adsorbent in Example 6.

[0028] Figure 3 This is a scanning electron microscope image of the magnetic porous monolithic adsorbent in Example 6.

[0029] Figure 4 This is a transmission electron microscope image of the magnetic porous monolithic adsorbent in Example 6.

[0030] Figure 5 This is a graph showing the service life of the magnetic porous monolithic adsorbent in Example 6.

[0031] Figure 6 These are the HPLC chromatograms of the four triazoles and two Cr complexes spiked with 100 ppb in Example 10, directly injected before extraction (a), after the spiked sample was extracted with the magnetic porous monolith (without a magnetic field) (b), and after the spiked sample was extracted with the magnetic porous monolith (with a magnetic field applied) (c). DETAILED DESCRIPTION

[0032] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention clearer and more understandable, the present invention is further described in detail below with reference to the accompanying drawings and embodiments.

[0033] Example 1

[0034] Synthesis of magnetic nanoparticles:

[0035] First, 5.4g of FeCl3·6H2O and 1.98g of FeCl2·4H2O were dissolved in 100mL of ultrapure water. The solution was placed in an 80°C water bath and stirred continuously for 2 hours. When the water bath temperature reached 60°C, 10mL of ethylenediamine was added, and nitrogen was continuously introduced during the reaction. After the reaction, the resulting Fe3O4 was washed with methanol, ultrapure water, and acetone, respectively, and then dissolved in 150mL of ultrapure water to obtain an Fe3O4 solution. The solution containing 1g of Fe3O4 particles was dispersed in 100mL of isopropanol, and 5mL of tetraethyl orthosilicate and 60mL of 25% ammonia were added. The reaction was allowed to proceed at room temperature for 12 hours to obtain Fe3O4@SiO2 particles. Mix Fe3O4@SiO2 (1 g), methanol (10 mL), triethylamine (1 mL) and 3-(isobutyleneoxy)propyltrimethoxysilane (1 mL) and shake on a shaker for 12 hours. This step can introduce double bonds on the particles. The particles are washed with methanol and dried at 60°C to obtain modified Fe3O4 nanoparticles.

[0036] Example 2

[0037] Preparation of magnetic porous monolithic adsorbent:

[0038] The synthetic reaction equation of magnetic porous monolithic adsorbent is as follows: Figure 1As shown, a prepolymerization solution was prepared using VAP and MAT as functional monomers, EDMA and DVB as crosslinkers, n-propanol and 1,4-butanediol as porogens, and AIBN as an initiator. The prepolymerization solution consisted of 10% functional monomers, 20% crosslinker, and 70% porogen, by mass. The functional monomers were 50% VAP and 50% MAT, the crosslinker was 40% EDMA and 60% DVB, and the porogen was 50% n-propanol and 50% 1,4-butanediol. The amount of AIBN added was 1.0 mg per 100 mg of prepolymerization solution, and the amount of magnetic nanoparticles added was 0.5 mg per 100 mg of prepolymerization solution. The mixed prepolymerization solution was poured into a tubular container, sealed, and reacted at 70°C for 10 hours. After the polymerization reaction was completed, the solution was rinsed with 1.0 mL of methanol.

[0039] Example 3

[0040] Preparation of magnetic porous monolithic adsorbent:

[0041] A prepolymerization solution was prepared using VAP and MAT as functional monomers, EDMA and DVB as crosslinkers, n-propanol and 1,4-butanediol as porogens, and AIBN as an initiator. The prepolymerization solution consisted of 20% functional monomers, 20% crosslinker, and 60% porogen, by mass. The functional monomers were 40% VAP and 60% MAT, the crosslinker was 60% EDMA and 40% DVB, and the porogen was 70% n-propanol and 30% 1,4-butanediol. The AIBN addition rate was 2.0 mg per 100 mg of prepolymerization solution, and the magnetic nanoparticles were 1.5 mg per 100 mg of prepolymerization solution. The mixed prepolymerization solution was poured into a tubular container, sealed, and reacted at 60°C for 24 hours. After the polymerization reaction was completed, the solution was rinsed with 2.0 mL of acetonitrile.

[0042] Example 4

[0043] Preparation of magnetic porous monolithic adsorbent:

[0044] A prepolymerization solution was prepared using VAP and MAT as functional monomers, EDMA and DVB as crosslinkers, n-propanol and 1,4-butanediol as porogens, and AIBN as an initiator. The prepolymerization solution consisted of 15% functional monomers, 25% crosslinker, and 60% porogen, by mass. The functional monomers were 30% VAP and 70% MAT, the crosslinker was 50% EDMA and 50% DVB, and the porogen was 40% n-propanol and 60% 1,4-butanediol. The amount of AIBN added was 1.5 mg per 100 mg of prepolymerization solution, and the amount of magnetic nanoparticles added was 1.0 mg per 100 mg of prepolymerization solution. The mixed prepolymerization solution was poured into a tubular container, sealed, and reacted at 80°C for 8 hours. After the polymerization reaction was completed, the solution was rinsed with 2.0 mL of methanol.

[0045] Example 5

[0046] Preparation of magnetic porous monolithic adsorbent:

[0047] A prepolymerization solution was prepared using VAP and MAT as functional monomers, EDMA and DVB as crosslinkers, n-propanol and 1,4-butanediol as porogens, and AIBN as an initiator. The prepolymerization solution consisted of 20% functional monomers, 10% crosslinker, and 70% porogen, by mass. The functional monomers were 60% VAP and 40% MAT, the crosslinkers were 30% EDMA and 70% DVB, and the porogens were 50% n-propanol and 50% 1,4-butanediol. The amount of AIBN added was 2.0 mg per 100 mg of prepolymerization solution, and the amount of magnetic nanoparticles added was 2.0 mg per 100 mg of prepolymerization solution. The mixed prepolymerization solution was poured into a tubular container, sealed, and reacted at 70°C for 24 hours. After the polymerization reaction was completed, the solution was rinsed with 4.0 mL of methanol.

[0048] Example 6

[0049] Preparation of magnetic porous monolithic adsorbent:

[0050] A prepolymerization solution was prepared using VAP and MAT as functional monomers, EDMA and DVB as crosslinkers, n-propanol and 1,4-butanediol as porogens, and AIBN as an initiator. The prepolymerization solution consisted of 16% functional monomers, 19% crosslinker, and 65% porogen, by mass. The functional monomers were 25% VAP and 75% MAT, the crosslinker was 50% EDMA and 50% DVB, and the porogen was 50% n-propanol and 50% 1,4-butanediol. The AIBN addition rate was 2.0 mg per 100 mg of prepolymerization solution, and the magnetic nanoparticles were 2.5 mg per 100 mg of prepolymerization solution. The mixed prepolymerization solution was poured into a tubular container, sealed, and reacted at 70°C for 12 hours. After the polymerization reaction was completed, the solution was rinsed with 5.0 mL of acetonitrile.

[0051] Figure 2 This is the infrared spectrum of the magnetic porous monolithic adsorbent prepared in this example, where 2936 cm -1 The absorption peak is the stretching vibration of the alkyl group, 1728 cm -1 The absorption peak is the characteristic peak of carbonyl in EDMA, 1638 cm -1 The absorption peak at 1458 cm is attributed to the stretching vibration of the C=C functional group. -1 The absorption peak at 1109 cm is attributed to the stretching vibration of the benzene ring. -1 and 1167cm -1 The absorption peak at 712 cm is attributed to the stretching vibration of CN of VAP and MAT. -1 The absorption peak at 573 cm is attributed to the stretching vibration of CF on MAT. -1 The absorption peak at corresponds to the stretching vibration of Fe-O. Figure 3 The scanning electron microscope image of the magnetic porous monolithic adsorbent prepared in this example shows a clear porous structure. Figure 4 This is a transmission electron microscope image of the magnetic porous monolithic adsorbent prepared in this example, in which the magnetic nanoparticles are uniformly dispersed in the porous monolithic material. Figure 5 This is a graph showing the service life of the magnetic porous monolithic adsorbent. After repeated adsorption and desorption for 120 times, the adsorption performance remains good.

[0052] Example 7

[0053] Preparation of magnetic porous monolithic adsorbent:

[0054] A prepolymerization solution was prepared using VAP and MAT as functional monomers, EDMA and DVB as crosslinkers, n-propanol and 1,4-butanediol as porogens, and AIBN as an initiator. The prepolymerization solution consisted of 4% functional monomers, 6% crosslinker, and 90% porogen, by mass. The functional monomers were 25% VAP and 75% MAT, the crosslinker was 75% EDMA and 25% DVB, and the porogen was 30% n-propanol and 70% 1,4-butanediol. The amount of AIBN added was 4.0 mg per 100 mg of prepolymerization solution, and the amount of magnetic nanoparticles added was 5.0 mg per 100 mg of prepolymerization solution. The mixed prepolymerization solution was poured into a tubular container, sealed, and reacted at 70°C for 18 hours. After the polymerization reaction was completed, the solution was rinsed with 10 mL of acetonitrile.

[0055] Example 8

[0056] Comparison of performance of magnetic porous monolithic adsorbents under different preparation conditions:

[0057] The porous monolithic adsorbents prepared in Examples 2 to 7 were used to enrich triazole pesticides and various chromium forms. A sample solution containing 100 μg / L of the target compounds was prepared. The target compounds included four triazole pesticides (triadimenol (TRN), myclobutanil (MYC), triadimefon (TRF), and hexaconazole (HEX)) and two chromium forms (Cr(III) and Cr(VI)). The specific extraction conditions were as follows: a sample volume of 3.0 mL, an adsorption flow rate of 0.10 mL / min, a desorption solvent volume of 100 μL of acetonitrile, a desorption flow rate of 0.06 mL / min, and no pH adjustment was performed on the sample solution. Under these conditions, the enrichment efficiency of the adsorbent for the target substance in Example 2 was 28.9% to 51.0%; in Example 3, it was 24.0% to 52.8%; in Example 4, it was 33.0% to 51.4%; in Example 5, it was 30.6% to 60.7%; in Example 6, it was 39.5% to 65.5%; and in Example 7, it was 35.9% to 57.1%. The porous monolithic adsorbent prepared in Example 6 showed the best enrichment performance for triazole pesticides and different forms of chromium.

[0058] Example 9

[0059] Application of magnetic field-assisted in-tube solid phase microextraction-chromatography online coupling device based on the adsorbent of the present invention:

[0060] The online coupling device consists of an extraction device and a chromatographic detection device. The extraction device includes two high-pressure constant-flow pumps, a six-way valve, and a capillary microextraction column containing a magnetic porous monolithic adsorbent. The chromatographic detection device includes a six-way valve, a quantitative loop, and a high-performance liquid chromatograph containing a high-pressure pump and a diode array detector. The two six-way valves are connected by PEEK tubing, and the online adsorption, desorption, and detection processes of the sample are achieved by switching the valve positions. The capillary microextraction column is wrapped with a magnetic coil that can be connected to a DC power supply. During the adsorption and desorption process, the magnetic coil generates a magnetic field of a certain strength and direction by controlling the magnitude and direction of the current. At this time, the magnetic nanoparticles in the capillary microextraction column are induced to produce a certain magnetic field gradient, which can improve the extraction efficiency of the target substance.

[0061] In order to meet the requirements of chromatographic separation and detection, ammonium pyrrolidine dithiocarbamate (APD) was added to the sample solution before extraction to react with Cr(III) and Cr(VI) to form Cr(III)-APD and Cr(VI)-APD complexes, respectively. The complexation reaction equation is shown below:

[0062]

[0063] During the adsorption process, the direction of the magnetic field in the capillary microextraction column is consistent with the flow direction of the sample solution, and the magnetic field strength is 20Gs. At the same time, 8.0mL of sample solution is input into the capillary microextraction column at a flow rate of 0.25mL / min to adsorb the target object; after the adsorption is completed, the direction of the magnetic field in the capillary microextraction column is reversed, and the magnetic field strength is 40Gs. 110μL of acetonitrile is input into the capillary microextraction column at a flow rate of 0.04mL / min to desorb the target object, and the eluent is stored in the quantitative loop; after the desorption is completed, the eluent is brought into the chromatographic column using the chromatographic mobile phase, and finally enters the diode array detector for measurement.

[0064] Example 10

[0065] An 8.0 mL water sample containing TRN, MYC, TRF, HEX, Cr(III), and Cr(VI) (containing 40 mg / L of the complexing agent APD) was prepared (each target compound was spiked at a concentration of 100 μg / L). Online extraction and detection were performed using the magnetic porous monolithic adsorbent prepared in Example 6 using the magnetic field-assisted in-tube solid-phase microextraction-chromatography online coupling apparatus described in Example 9.

[0066] The instruments used for chromatographic analysis were HPLC system and DAD detector (Model 1260, Agilent, USA). The HPLC conditions included a chromatographic column, mobile phase A, mobile phase B, elution procedure, and detection wavelength. The chromatographic column was a ThermoHypersil BDS C18 column (250 mm × 4.6 mm id, 5 μm particle size), mobile phase A was ultrapure water, mobile phase B was acetonitrile, and the gradient elution was: 0-11.0 min, 53% B; 11.0-15.0 min, 53%-70% B; 15.0-18.0 min, 70% B; 18.0-22.0 min, 70%-53% B; 22.0-25.0 min, 53% B; the injection volume was 110 μL, the flow rate was 1.0 mL / min, the detection wavelength for TRN, MYC, TRF, and HEX was 223 nm, and the detection wavelength for Cr(III)-APD and Cr(VI)-APD was 254 nm. Figure 6 High-performance liquid chromatograms of four triazoles and two chromium complexes spiked at 100 ppb at 223 nm, directly before extraction (a), after extraction with the magnetic porous monolith (without a magnetic field) (b), and after extraction with the magnetic porous monolith (with a magnetic field applied) (c). Without a magnetic field, the enrichment efficiency for the target compounds ranged from 46.2% to 75.3%. With the application of a magnetic field, the peak heights of the target compounds increased significantly, raising the enrichment efficiency to 80.5% to 98.0%.

Claims

1. A method for preparing a magnetic porous monolithic adsorbent capable of simultaneously enriching triazole pesticides, Cr(III) and Cr(VI), characterized in that: The following steps are involved: 1) functional monomers, cross-linking agents, porogens, initiators and magnetic nanoparticles are mixed in proportion and ultrasonically mixed into a uniform solution; 2) injecting the prepolymer solution mixed in step 1) into a container, sealing it, and initiating a polymerization reaction at a certain temperature; 3) After the polymerization reaction is completed, rinse it with a certain volume of methanol or acetonitrile, and rinse it with methanol or acetonitrile before use to activate it; The functional monomers are ethylene boric anhydride pyridine solvate (VAP) and 1-allyl-3-methylimidazole bis(trifluoromethanesulfonyl)imide salt (MAT); The cross-linking agents are ethylene glycol dimethacrylate (EDMA) and divinylbenzene (DVB); The porogens are n-propanol and 1,4-butanediol.

2. The method for preparing a magnetic porous monolithic adsorbent capable of simultaneously enriching triazole pesticides, Cr(III) and Cr(VI) according to claim 1, characterized in that: The added amount of the VAP and the MAT is 10% to 30% of the total mass of the prepolymerization solution, and the mass ratio of the VAP to the MAT is 1:4 to 4:

1.

3. The method for preparing a magnetic porous monolithic adsorbent capable of simultaneously enriching triazole pesticides, Cr(III) and Cr(VI) according to claim 1, characterized in that: The added amount of the EDMA and DVB is 10% to 30% of the total mass of the prepolymerization solution, and the mass ratio of the EDMA to DVB is 1:3 to 3:

1.

4. The method for preparing a magnetic porous monolithic adsorbent capable of simultaneously enriching triazole pesticides, Cr(III) and Cr(VI) according to claim 1, characterized in that: The added amount of the n-propanol and 1,4-butanediol is 40% to 90% of the total mass of the prepolymerization solution, and the mass ratio of the n-propanol to 1,4-butanediol is 1:3 to 3:

1.

5. The method for preparing a magnetic porous monolithic adsorbent capable of simultaneously enriching triazole pesticides, Cr(III) and Cr(VI) according to claim 1, characterized in that: The initiator is azobisisobutyronitrile (AIBN); the mass of AIBN added is 0.2-4.0 mg / 100 mg of the prepolymerization solution.

6. The method for preparing a magnetic porous monolithic adsorbent capable of simultaneously enriching triazole pesticides, Cr(III) and Cr(VI) according to claim 1, characterized in that: The magnetic nanoparticles are modified Fe3O4 nanoparticles; the mass of the magnetic nanoparticles added is 0.5-5.0 mg / 100 mg of the prepolymer solution.

7. The method for preparing a magnetic porous monolithic adsorbent capable of simultaneously enriching triazole pesticides, Cr(III) and Cr(VI) according to claim 1, characterized in that: In step 2), the polymerization reaction temperature is 60-80° C., and the polymerization reaction time is 8-24 hours; in step 3), the certain volume is 1.0-10 mL.

8. A magnetic porous monolithic adsorbent capable of simultaneously enriching triazole pesticides, Cr(III) and Cr(VI), characterized in that: Prepared by the preparation method according to any one of claims 1 to 7.

9. The use of a magnetic porous monolithic adsorbent capable of simultaneously enriching triazole pesticides, Cr(III) and Cr(VI) as claimed in claim 8, characterized in that: The magnetic porous monolithic adsorbent is used to pre-treat samples containing triazole pesticides, Cr(III) and Cr(VI) by adsorption, followed by desorption, and finally the triazole pesticides and different forms of Cr are simultaneously analyzed by a chromatographic detection method.

10. The use according to claim 9, characterized in that: In the pre-adsorption treatment, a complexing agent is used to convert Cr(III) and Cr(VI) into metal-organic complexes that can be detected by HPLC-DAD; ultrapure water and acetonitrile are used as mobile phases, and a gradient elution program is set: 0-11.0 min, 53% acetonitrile; 11.0-15.0 min, 53%-70% acetonitrile; 15.0-18.0 min, 70% acetonitrile; 18.0-22.0 min, 70%-53% acetonitrile; 22.0~25.0min, 53% acetonitrile, simultaneous detection of triazole pesticides and different forms of Cr can be achieved.

Citation Information

Patent Citations

  • Preparation method for porous integral extracting medium based on boron affinity interaction

    CN104610498A

  • Preparation method of porous adsorbent on basis of multifunctional monomers and cross-linking agents

    CN107383262A

  • Oxygen separating agent and preparation trereof

    JP1992358537A