Method for preparing propane dehydrogenation catalyst by using ACC wood preservative wastewater

Through precipitation treatment and composite support technology, a cheap and stable propane dehydrogenation catalyst was prepared, which solved the problems of environmental harm of chromium catalysts and the high cost of ACC wastewater treatment, and achieved efficient preparation of propane dehydrogenation catalysts and ACC wastewater. Secondary use.

CN119056461AActive Publication Date: 2024-12-03PETROCHINA CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310653543.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-06-02
Publication Date
2024-12-03
Estimated Expiration
2043-06-02

Smart Images

  • Figure CN119056461A_ABST
    Figure CN119056461A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a propane dehydrogenation catalyst by using ACC wood preservative wastewater, which comprises the following steps: after the ACC wood preservative wastewater is subjected to precipitation treatment, taking supernatant liquid, filtering to remove impurities, then concentrating to a solution which is in a saturated state at normal pressure and 75-85 DEG C, and adjusting the pH value to be less than or equal to 1 to obtain steeping liquor; under the stirring state, a carrier is added into the impregnation liquid for impregnation, the impregnated carrier is dried and roasted in the air or nitrogen atmosphere, and the propane dehydrogenation catalyst is obtained, the carrier is a composite porous material formed by an inorganic porous material and a pore forming agent, or an inorganic porous material containing 3wt%-4wt% of nickel. In the catalyst prepared by the method for preparing the propane dehydrogenation catalyst by using the ACC wood preservative wastewater, both chromium ions and copper ions are derived from the ACC wood preservative wastewater, and the preparation cost of the propane dehydrogenation catalyst is reduced while the industrial wastewater is secondarily utilized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the fields of environment and petrochemical industry, and in particular to a method for preparing a propane dehydrogenation catalyst by utilizing ACC wood preservative wastewater. Background Art

[0002] With the beginning of the shale oil and gas revolution in North America, the overproduction of propane in the global chemical market has become an increasingly significant trend. In order to consume the excess propane and convert it into propylene with higher industrial added value, the propane dehydrogenation industry (PDH) has received unprecedented attention.

[0003] At present, there are four main propane dehydrogenation processes, among which the Oleflex process of Universal Oil Products (UOP) based on Pt-based catalysts and the Lummus process based on Cr-based catalysts are the most widely used processes. However, Pt-based catalysts have the characteristics of high requirements for raw material purity, easy agglomeration and deactivation, and high prices. Therefore, chromium-based catalysts with high toxicity have always occupied a certain market space. For example, Chinese patent document CN112403458A discloses a dual-active center propane dehydrogenation catalyst, including a carrier and an active component loaded on the carrier, wherein the carrier is a non-metallic carbon material, and the active component is a metal chromium oxide. Chinese patent document CN115501871A discloses a propane dehydrogenation catalyst, including: alumina containing group IVB elements as a carrier, Cr or its oxide as an active component, and group IA and / or group IIA elements or their oxides as an auxiliary component; wherein the catalyst passes the TPR test, and alloy peaks of group IVB elements and active component Cr elements appear in the range of 380 to 580°C.

[0004] It is reported that the main active site in chromium-based catalysts is Cr in Cr2O3. 6+ Cr 5+ It has a great impact on the health of aquatic plants and animals in natural water bodies, as well as humans and livestock. In order to alleviate the above problems, many research institutions at home and abroad have studied a variety of advanced adsorption materials to adsorb heavy metal ions such as high-valent metal chromium in water, thereby preventing heavy metal ions such as chromium and copper from irreversibly damaging the natural water environment.

[0005] On the other hand, after preliminary market research, it was found that acid copper chromate (ACC) wood preservative is one of the most widely used wood preservatives. Because the preservative contains a large amount of chromium ions and copper ions, the heavy metal ions in it need to be treated before discharge. At present, the general treatment method for ACC wastewater needs to go through four steps: 1. Pretreatment: Pretreatment mainly includes solid-liquid separation, precipitation, filtration and other methods to separate suspended matter, silt and other impurities in the wastewater and reduce the turbidity of the wastewater. For example, sedimentation tanks, filters and other equipment can be used for treatment. Neutralization reaction: The pH value in the wastewater may affect the subsequent treatment process, so neutralization treatment is required. The pH value of the wastewater can be adjusted to a moderate range by adding acid or alkali. 2. Chemical precipitation: Use chemical reactions to generate water-insoluble precipitates to settle ACC wood preservatives and other harmful substances in the wastewater. Commonly used chemical precipitants include aluminum hydroxide, iron hydroxide, etc. 3. Deep treatment: After the above treatment, the wastewater may still have certain residual pollutants. Deep treatment technologies, such as ultrafiltration, nanofiltration, reverse osmosis and other methods, can be used to further improve the treatment effect of wastewater. 4. Wastewater recycling or wastewater discharge: After the above treatment, the wastewater can meet certain water quality standards and can be considered for recycling, such as for flushing, greening, etc., to reduce water resource waste; or the treated wastewater can be discharged to the corresponding discharge port on the premise of ensuring that the wastewater meets the relevant national emission standards. However, the above treatment process is time-consuming and has a relatively high economic cost. Therefore, the treatment of heavy metal ions in ACC preservative wastewater has always been a problem that needs to be solved urgently.

[0006] If the toxic hexavalent chromium in ACC wastewater can be used for the preparation of catalysts, it will be of great significance for the reuse of ACC wastewater. Summary of the invention

[0007] The purpose of the present invention is to provide a method for preparing a propane dehydrogenation catalyst by using ACC wood preservative wastewater. The method not only prepares a cheap Cr-based propane dehydrogenation catalyst, but also takes into account the treatment of hazardous chemicals, thereby solving the problem of secondary utilization of ACC wood preservative wastewater containing heavy metal ions.

[0008] To achieve the above object, the present invention provides a method for preparing a propane dehydrogenation catalyst using ACC wood preservative wastewater, comprising the following steps:

[0009] Pretreatment: At room temperature, the ACC wood preservative wastewater is subjected to sedimentation treatment, the upper clear liquid is filtered to remove impurities, and then concentrated to a saturated solution at normal pressure and 75-85°C, and the pH is adjusted to ≤1 to obtain an impregnation solution;

[0010] Impregnation: adding the carrier to the impregnation solution for impregnation at 75-85° C. under stirring, and drying and calcining the impregnated carrier to obtain a propane dehydrogenation catalyst;

[0011] Wherein, the carrier is a composite porous material formed by an inorganic porous material and a pore-forming agent, or an inorganic porous material containing 3wt% to 4wt% nickel.

[0012] Optionally, in the method for preparing a propane dehydrogenation catalyst using ACC wood preservative wastewater provided by the present invention, the calcination atmosphere is air, hydrogen or nitrogen.

[0013] In the method for preparing propane dehydrogenation catalyst using ACC wood preservative wastewater provided by the present invention, the inorganic porous material containing 3wt% to 4wt% nickel means that the mass of the inorganic porous material containing nickel is 100%, wherein the content of nickel is 3wt% to 4wt%.

[0014] In the method for preparing propane dehydrogenation catalyst using ACC wood preservative wastewater provided by the present invention, the purpose of adjusting the pH of the saturated solution to ≤ 1 is to ensure that the valence of the metal ions maintains a certain high valence state after subsequent roasting. 6+ ratio, thereby ensuring the catalytic activity of the final catalyst.

[0015] In the method for preparing propane dehydrogenation catalyst using ACC wood preservative wastewater provided by the present invention, the purpose of filtering the supernatant after the ACC wood preservative wastewater is to remove impurities, floating materials, sawdust and other substances in the ACC wood preservative wastewater, so as to ensure the safety and feasibility of subsequent use in preparing the dehydrogenation catalyst.

[0016] In the method for preparing propane dehydrogenation catalyst using ACC wood preservative wastewater provided by the present invention, the concentration is limited to a saturated solution at normal pressure and 75-85°C in order to prevent the precipitation of metal salts and affect the subsequent impregnation effect. If the limited temperature is too low or too high, the metal salt content in the saturated solution will be low, and the activity of the obtained catalyst will be poor.

[0017] Optionally, in the method for preparing a propane dehydrogenation catalyst using ACC wood preservative wastewater provided by the present invention, it is necessary to ensure that no solute precipitates in the saturated ACC wood preservative wastewater during the impregnation process, and the present invention recommends that the impregnation be performed in a rotary evaporator; preferably, the impregnation time is 30 to 60 minutes. By limiting the impregnation step to be performed in a rotary evaporator, combined with the limitation of the impregnation temperature and time, the precipitation of solutes during the impregnation process can be prevented, thereby affecting the effect of the impregnation.

[0018] Optionally, in the method for preparing a propane dehydrogenation catalyst using ACC wood preservative wastewater provided by the present invention, in the pretreatment step, the concentration temperature is 75-85°C.

[0019] Optionally, in the method for preparing a propane dehydrogenation catalyst using ACC wood preservative wastewater provided by the present invention, the main heavy metal ions in the ACC wood preservative wastewater include chromium ions and copper ions, and the presence of copper ions can help chromium ions to be adsorbed on the surface of the carrier. Chromium ions can also help copper ions to be adsorbed on the surface of the carrier, and the two promote adsorption of each other.

[0020] Optionally, in the method for preparing a propane dehydrogenation catalyst using ACC wood preservative wastewater provided by the present invention, the inorganic porous material is selected from at least one of macroporous alumina, high-purity alumina, mesoporous silica, zinc oxide, zirconium oxide, boron nitride and pseudo-boehmite.

[0021] Optionally, in the method for preparing a propane dehydrogenation catalyst using ACC wood preservative wastewater provided by the present invention, the composite porous material is prepared by a wet mixing method of an inorganic porous material and a pore-forming agent, and preferably the mass ratio of the inorganic porous material to the pore-forming agent is 2 to 5: 1. The process parameters of the wet mixing method can be conventional ones in the industry and are not specifically limited.

[0022] Optionally, in the method for preparing a propane dehydrogenation catalyst using ACC wood preservative wastewater provided by the present invention, the pore-forming agent can be selected from conventional ones in the industry. For cost considerations, the pore-forming agent recommended by the present invention is selected from sesbania gum and / or CMC (sodium carboxymethyl cellulose).

[0023] Optionally, in the method for preparing a propane dehydrogenation catalyst using ACC wood preservative wastewater provided by the present invention, the inorganic porous material containing 3wt% to 4wt% nickel is obtained by impregnating the inorganic porous material in a nickel nitrate solution, aging, sintering at 700 to 750°C for 5 to 6 hours, and naturally cooling to room temperature. If the nickel loading requirement cannot be met by one impregnation, after sintering, the steps of impregnation, drying and roasting can be repeated, and the impregnation can be repeated multiple times until the required nickel loading requirement is met.

[0024] Optionally, in the method for preparing a propane dehydrogenation catalyst using ACC wood preservative wastewater provided by the present invention, the aging procedure is: first maintain at 80-90° C. for 3-4 hours, then immediately heat to 120-140° C. and maintain for 4-12 hours;

[0025] The solvent of the nickel nitrate solution can be deionized water, and the concentration is not specifically limited, which does not affect the impregnation result. When the concentration is dilute, the loading requirement can be achieved by multiple impregnations. The concentration of the nickel nitrate recommended by the present invention is 0.001 mol / ml to 0.01 mol / ml.

[0026] Optionally, in the method for preparing a propane dehydrogenation catalyst using ACC wood preservative wastewater provided by the present invention, concentrated nitric acid is used to adjust the pH of the saturated solution.

[0027] Optionally, in the method for preparing a propane dehydrogenation catalyst using ACC wood preservative wastewater provided by the present invention, the calcination temperature is 650 to 850° C. and the calcination time is 7 to 10 hours.

[0028] Optionally, in the method for preparing a propane dehydrogenation catalyst using ACC wood preservative wastewater provided by the present invention, the drying is vacuum drying, first drying at 75-85° C. for 3-4 hours, and then drying at 120-140° C. for 12-14 hours.

[0029] The propane dehydrogenation catalyst prepared by the method for preparing a propane dehydrogenation catalyst by using ACC wood preservative wastewater provided by the present invention has a lateral compression strength of 174-200 N / cm.

[0030] Compared with the prior art, the present invention has the following advantages:

[0031] In the propane dehydrogenation catalyst prepared by the method for preparing a propane dehydrogenation catalyst by using ACC wood preservative wastewater provided by the present invention, chromium ions and copper ions are both derived from ACC wood preservative wastewater, and while industrial wastewater is reused for a second time, the preparation cost of the propane dehydrogenation catalyst and the environmental pressure of ACC wood preservative wastewater are reduced, and the method is easy to operate and has a simple process. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 A schematic diagram of a method for preparing a propane dehydrogenation catalyst using ACC wood preservative wastewater provided by the present invention;

[0033] Among them, 1-filter; 2-heating furnace; 3-evaporating dish; 4-rotary evaporating dish; 5-rotary evaporator; 6-molded catalyst particles. DETAILED DESCRIPTION

[0034] The present invention is described in detail below by way of examples. It is necessary to point out that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Those skilled in the art in this field can make some non-essential improvements and adjustments to the present invention based on the above content of the present invention.

[0035] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0036] The heavy metal ions such as chromium and copper contained in ACC wood preservative wastewater cause irreversible damage to the natural water environment. Therefore, the heavy metal ions in it need to be treated before discharge. The current common ACC wastewater treatment method requires four steps. Not only is the treatment process time-consuming, but the economic cost is relatively high. In order to reduce the pressure on the environment caused by ACC wood preservative wastewater and effectively utilize the heavy metal ions therein, the inventor creatively proposed to use the heavy metal ions in ACC wood preservative wastewater as active ingredients in propane dehydrogenation catalysts. However, due to the low concentration of heavy metal ions in ACC wood preservative wastewater and the presence of many other impurities, in order to ensure its safety and feasibility in the preparation of dehydrogenation catalysts, ACC wood preservative wastewater needs to be effectively pretreated.

[0037] The inventors have found that, although the neutralization pretreatment method can effectively remove impurities in ACC wood preservative wastewater, a large amount of acid or alkali needs to be added, which increases the treatment cost; and the large amount of sludge generated further increases the treatment cost and environmental pressure; more seriously, due to the large fluctuation of pH in the wastewater, it is difficult to achieve a sustained and stable neutralization effect, resulting in unstable acid-base regulation, which directly affects the preparation and catalytic effect of subsequent catalysts. The price of adsorbents (such as activated carbon) is relatively high when using adsorption pretreatment, and the adsorbent is easy to saturate and needs to be replaced regularly. The used adsorbent contains a large amount of pollutants and needs to be safely disposed of to prevent secondary pollution. The treatment process is complicated and the cost is high. After in-depth research, the inventors found that by adopting the precipitation method, the dust and sawdust coated with preservatives can be removed from the ACC wastewater, and then the supernatant can be filtered and concentrated into a saturated solution at a specific temperature, and the pH is adjusted to ≤1. The entire pretreatment process does not introduce any new metal atoms or non-metal atoms, and effectively increases the concentration of heavy metal ions in the ACC wastewater, providing a certain guarantee for the activity of the catalyst finally obtained. Moreover, adjusting the pH after precipitation concentration increases the stability of acid-base regulation and can effectively prevent the presence of metal valence states on the carrier surface after impregnation due to an increase in pH, thereby affecting the activity of the catalyst.

[0038] The dehydrogenation catalyst must have good dispersibility, activity and stability to ensure its dehydrogenation reaction effect. In order to ensure that the prepared dehydrogenation catalyst has good dispersibility, activity and stability, it is necessary to use a suitable carrier and method for preparation. The copper content in the catalyst prepared from ACC wood preservative wastewater is relatively high. This is because the d electrons of copper tend to be saturated. The high content of copper makes the dehydrogenation activity of the catalyst not very strong, but the high content of copper can disperse the main dehydrogenation active center Cr. Because the chromium oxide cluster is the main active site of the catalyst, when the size of the active site becomes larger, the selectivity of the active site and the side reactions such as carbon deposition and cracking will increase accordingly. Therefore, it is necessary to distribute elements with weaker dehydrogenation activity on the carrier surface to improve the stability of the catalyst, reduce carbon deposition, and improve the selectivity of the catalyst for propylene. However, a single inorganic carrier has poor dispersion of chromium metal and does not have an electronic regulation effect on the main active site.

[0039] In order to make up for the shortcomings of conventional inorganic porous materials as dehydrogenation catalyst carriers, the inventors have found through further in-depth research: 1) The above shortcomings can be made up by loading a certain amount of Ni element on the surface of the inorganic porous material. The reason is that Ni forms a spinel structure inside the inorganic porous material, in which the nickel element presents a four-coordinated positive divalent structure, has a certain dehydrogenation activity, and assists the main active site to complete the dehydrogenation process. Due to the presence of the spinel structure, the carbon deposition of the catalyst will be reduced, and its stability and hardness will be improved, thereby ensuring the robustness of the industrial dehydrogenation catalyst in harsh environments. From the perspective of electronic effects, the introduction of metallic nickel is equivalent to doping with an auxiliary agent, which plays a role in supplying electrons to chromium. The surface of chromium oxide is electron-rich, which is conducive to the desorption of propylene, thereby reducing carbon deposition and improving the selectivity of propylene. 2) The composite carrier formed by pore-forming agent and inorganic porous material can also make up for the above shortcomings. Since propane dehydrogenation is a gas-solid phase catalysis in heterogeneous catalysis, the addition of pore-forming agent can significantly increase the surface area of ​​the inorganic porous material with a small specific surface area, thereby forming developed pores, improving the carrier's anti-coking ability and reaction stability, and at the same time, significantly improving the regeneration ability of the catalyst.

[0040] In summary, under the premise of ensuring that the dehydrogenation catalyst prepared by using heavy metal ions in ACC wood preservative wastewater has good dispersibility, activity and stability, it is necessary to first effectively pretreat the ACC wood preservative wastewater, and then select a suitable carrier and method for effective loading. Therefore, the factors affecting the preparation of dehydrogenation catalysts using ACC wastewater are many and complex. After comprehensive and in-depth research, the inventors finally determined that the pretreatment method including sequential precipitation, filtration and concentration into a saturated solution at 75-85°C, and adjusting the pH ≤ 1, combined with a specific carrier and impregnation loading method, can ensure the application effect of the prepared catalyst.

[0041] In order to further illustrate the technical solution of the present invention, specific examples are provided below. It should be noted that the following specific implementation scheme does not constitute a limitation on the protection scope of the present invention.

[0042] For the convenience of comparison, the raw materials involved in the catalyst preparation process in the following specific examples are all analytical grade (AR). Nickel nitrate was purchased from Aladdin Reagent Company; the rotary evaporation equipment required for the experiment was produced by Ranhui Instrument Company; Tianqing gum was purchased from Beijing Mining Research Institute; and pseudo-boehmite was purchased from Chalco Shandong New Materials Co., Ltd. and Chalco Shanxi Co., Ltd.

[0043] Example 1

[0044] This embodiment provides a method for preparing a propane dehydrogenation catalyst using ACC wood preservative wastewater. Part of the pretreatment and impregnation process is as follows: Figure 1 As shown, the specific steps include:

[0045] Pretreatment: at room temperature, the ACC wood preservative wastewater is allowed to settle, and then the supernatant is filtered using a filter 1, and the obtained filtrate is placed in an evaporating dish 3, and heated to 75-85°C using a heating furnace 2 under normal pressure to concentrate into a saturated solution at 80°C, and then the pH value is tested using an acidic pH test paper, and concentrated nitric acid is slowly added to adjust the pH of the saturated solution to ≤1, to obtain an impregnation solution;

[0046] Carrier: Pseudo-boehmite from Chalco Shandong New Materials Co., Ltd., sesbania gum from Beijing Mining Research Institute and macroporous alumina from Chalco Shandong New Materials Co., Ltd. were dry mixed in a mass ratio of 3:1:0.2. After mixing evenly, deionized water was added and stirred evenly to form a viscous state. Then, the mixture was put into a kneading machine and fully kneaded at a speed of 900r / min. Then, the mixture was extruded into strips in an extruder with an orifice diameter of 2mm. The formed samples were dried and calcined to obtain catalyst carriers. The drying procedure was: first kept at 60°C for 4 hours, then kept at 120°C for 4 hours; the calcination procedure was: heating from room temperature to 750°C at a rate of 5°C / min, maintained for 8 hours, and then naturally cooled to room temperature.

[0047] Impregnation: Place the above catalyst carrier in a rotary evaporation dish 4 and preheat it to 70-80°C, then add the above impregnation solution and impregnate at 75-85°C for 30 minutes with equal volume under the stirring action of the rotary evaporator 5. Place the obtained shaped catalyst particles 6 in a watch glass and then dry them in a vacuum oven: first maintain at 80°C for 3 hours, then immediately heat to 120°C and maintain for 12 hours; then immediately place the dried sample in a muffle furnace for calcination: heat to about 800°C in an air atmosphere and maintain for 7 hours, then naturally cool to room temperature to obtain a propane dehydrogenation catalyst.

[0048] Comparative Example 1-1

[0049] This comparative example 1-1 is basically the same as Example 1, except that nickel is loaded on the carrier used. The preparation process of the carrier used in this comparative example is as follows:

[0050] The preparation method of the intermediate carrier is the same as the preparation method of the carrier in Example 1;

[0051] The intermediate carrier was immersed in a 0.006 mol / ml nickel nitrate aqueous solution, then maintained at 80°C for 3 hours, then dried at 120°C for 5 hours, and finally sintered at 700°C for 5 hours. The nickel content was detected to be 2wt%, thus obtaining a catalyst carrier containing 2wt% nickel.

[0052] The nickel loaded in this comparative example is used as a promoter of the chromium / copper catalyst to improve the initial catalytic activity and stability of the catalyst.

[0053] Comparative Example 1-2

[0054] This comparative example 1-2 is basically the same as Example 1, except that nickel is loaded on the carrier used. The preparation process of the carrier used in this comparative example is as follows:

[0055] The preparation method of the intermediate carrier is the same as the preparation method of the carrier in Example 1;

[0056] The intermediate carrier was immersed in a 0.01 mol / ml nickel nitrate aqueous solution, then maintained at 80°C for 3 hours, then dried at 120°C for 8 hours, and finally sintered at 700°C for 5 hours. The nickel content was detected to be 3.5wt%, thus obtaining a catalyst carrier containing 3.5wt% nickel.

[0057] The nickel loaded in this comparative example is also used as an auxiliary agent for the chromium / copper catalyst to improve the initial catalytic activity and stability of the catalyst.

[0058] Example 2

[0059] This embodiment provides a method for preparing a propane dehydrogenation catalyst using ACC wood preservative wastewater, which specifically includes the following steps:

[0060] Pretreatment: At room temperature, the ACC wood preservative wastewater was allowed to settle, and then the supernatant was filtered. The obtained filtrate was concentrated at normal pressure and 75-85°C to a saturated solution at 80°C. Then, the pH value was tested using an acidic pH test paper, and concentrated nitric acid was slowly added to adjust the pH of the saturated solution to ≤1 to obtain an impregnation solution.

[0061] Support: High-purity mesoporous silica was immersed in a 0.008 mol / ml nickel nitrate aqueous solution, then maintained at 80°C for 3 hours, then maintained at 120°C for 8 hours for aging, and finally sintered at 700°C for 5 hours. The nickel content was detected to be 3wt%, thus obtaining a high-purity mesoporous silica support containing 3wt% nickel.

[0062] Impregnation: The catalyst carrier is placed in the impregnation solution and impregnated in a rotary evaporator at an equal volume for 60 minutes at 75-85°C. The impregnated carrier is placed in a watch glass and dried in a vacuum oven: first maintained at 80°C for 3 hours, then immediately heated to 120°C and maintained for 12 hours; then the dried sample is immediately placed in a muffle furnace for calcination: heated to about 800°C in an air atmosphere and maintained for 7 hours, then naturally cooled to room temperature to obtain a propane dehydrogenation catalyst.

[0063] Comparative Example 2

[0064] This comparative example is basically the same as Example 2, except that the nickel content loaded on the high-purity mesoporous silica carrier used is different. In this comparative example, the nickel content loaded on the high-purity mesoporous silica carrier is 2.5wt%. The specific operation is as follows:

[0065] High-purity mesoporous silica was immersed in a 0.004 mol / ml nickel nitrate aqueous solution, then maintained at 80°C for 3 hours, then maintained at 120°C for 12 hours for aging, and finally sintered at 700°C for 5 hours. The nickel content was detected to be 2.5wt%, thus obtaining a high-purity mesoporous silica carrier containing 2.5wt% nickel.

[0066] Example 3

[0067] This embodiment provides a method for preparing a propane dehydrogenation catalyst using ACC wood preservative wastewater, which specifically includes the following steps:

[0068] Pretreatment: At room temperature, the ACC wood preservative wastewater was allowed to settle, and then the supernatant was filtered. The obtained filtrate was concentrated at normal pressure and 75-85°C to a saturated solution at 80°C. Then, the pH value was tested using an acidic pH test paper, and concentrated nitric acid was slowly added to adjust the pH of the saturated solution to ≤1 to obtain an impregnation solution.

[0069] Support: The zirconium oxide was immersed in a 0.08 mol / ml nickel nitrate aqueous solution, then maintained at 80°C for 3 hours, then maintained at 120°C for 12 hours for aging, and finally sintered at 700°C for 5 hours. The nickel content was detected to be 3wt%, thus obtaining a zirconium oxide support containing 3wt% nickel.

[0070] Impregnation: The catalyst carrier is placed in the impregnation solution and impregnated in a rotary evaporator at an equal volume for 40 minutes at 75-85°C. The impregnated carrier is placed in a watch glass and dried in a vacuum oven: first maintained at 80°C for 3 hours, then immediately heated to 120°C and maintained for 12 hours; then the dried sample is immediately placed in a muffle furnace for calcination: heated to 800°C in a nitrogen atmosphere and maintained for 7 hours, then naturally cooled to room temperature to obtain a propane dehydrogenation catalyst.

[0071] Comparative Example 3

[0072] This comparative example 3 is basically the same as Example 3, except that: the atmosphere during calcination in the impregnation step is different. In this comparative example, the dried sample is immediately placed in a muffle furnace for calcination: the temperature is raised to about 800°C in an argon atmosphere and maintained for 7 hours, and then naturally cooled to room temperature to obtain a propane dehydrogenation catalyst.

[0073] Example 4

[0074] This embodiment provides a method for preparing a propane dehydrogenation catalyst using ACC wood preservative wastewater, which specifically includes the following steps:

[0075] Pretreatment: At room temperature, the ACC wood preservative wastewater was allowed to settle, and then the supernatant was filtered. The obtained filtrate was concentrated at normal pressure and 75-85°C to a saturated solution at 80°C. Then, the pH value was tested using an acidic pH test paper, and concentrated nitric acid was slowly added to adjust the pH of the saturated solution to ≤1 to obtain an impregnation solution.

[0076] Carrier: Pseudo-boehmite from Zibo Hengyi Co., Ltd., sesbania gum from Beijing Mining Research Institute and macroporous alumina from Zibo Hengyi Co., Ltd. were dry mixed in a mass ratio of 3:1:0.2. After mixing evenly, deionized water was added and stirred evenly to form a viscous state. Then, the mixture was put into a kneading machine and fully kneaded at a speed of 900r / min. Then, the mixture was extruded into strips in an extruder with an orifice diameter of 2mm. The formed samples were dried and calcined to obtain catalyst carriers. The drying procedure was: first kept at 60°C for 4 hours, then kept at 120°C for 4 hours; the calcination procedure was: heating from room temperature to 750°C at a rate of 5°C / min, maintained for 8 hours, and then naturally cooled to room temperature.

[0077] Impregnation: Place the catalyst carrier in the above-mentioned impregnation solution and immerse it in an equal volume in a rotary evaporator at 75-85°C for 55 minutes. Place the impregnated carrier in a watch glass and put it into a vacuum oven for drying: first maintain it at 80°C for 3 hours, then immediately heat it to 120°C and maintain it for 12 hours; then immediately place the dried sample in a muffle furnace for calcination: heat it to about 800°C in an air atmosphere and maintain it for 7 hours, then naturally drop to room temperature to obtain a propane dehydrogenation catalyst.

[0078] Example 5

[0079] This embodiment provides a method for preparing a propane dehydrogenation catalyst using ACC wood preservative wastewater, which specifically includes the following steps:

[0080] Pretreatment: At room temperature, the ACC wood preservative wastewater was allowed to settle, and then the supernatant was filtered. The obtained filtrate was concentrated at normal pressure and 75-85°C to a saturated solution at 80°C. Then, the pH value was tested using an acidic pH test paper, and concentrated nitric acid was slowly added to adjust the pH of the saturated solution to ≤1 to obtain an impregnation solution.

[0081] Carrier: Chalco Shanxi pseudo-boehmite and pore-forming agent CMC are dry-mixed at a mass ratio of 2.5:1. After mixing evenly, deionized water is added and stirred evenly to form a viscous state. Then, the mixture is put into a kneading machine and fully kneaded at a speed of 900r / min. Then, the mixture is extruded into strips in an extruder with an orifice diameter of 2mm. The formed sample is dried and calcined to obtain a catalyst carrier. The drying procedure is: first keep at 60°C for 4 hours, then keep at 120°C for 4 hours; the calcination procedure is: heat up from room temperature to 750°C at a rate of 5°C / min, maintain for 8 hours, and then naturally drop to room temperature.

[0082] Impregnation: Place the catalyst carrier in the above-mentioned impregnation solution and immerse it in an equal volume in a rotary evaporator at 75-85°C for 35 minutes. Place the impregnated carrier in a watch glass and put it in a vacuum oven for drying: first maintain it at 80°C for 3 hours, then immediately heat it to 120°C and maintain it for 12 hours; then immediately place the dried sample in a muffle furnace for calcination: heat it to about 800°C in an air atmosphere and maintain it for 7 hours, then naturally drop to room temperature to obtain a propane dehydrogenation catalyst.

[0083] Example 6

[0084] This embodiment provides a method for preparing a propane dehydrogenation catalyst using ACC wood preservative wastewater, which specifically includes the following steps:

[0085] Pretreatment: At room temperature, the ACC wood preservative wastewater was allowed to settle, and then the supernatant was filtered. The obtained filtrate was concentrated at normal pressure and 75-85°C to a saturated solution at 80°C. Then, the pH value was tested using an acidic pH test paper, and concentrated nitric acid was slowly added to adjust the pH of the saturated solution to ≤1 to obtain an impregnation solution.

[0086] Support: High-purity mesoporous silica was immersed in a 0.01 mol / ml nickel nitrate aqueous solution, then maintained at 90°C for 3 hours, then maintained at 130°C for 6 hours for aging, and finally sintered at 750°C for 5.5 hours. The nickel content was detected to be 3.5wt%, thus obtaining a high-purity mesoporous silica support containing 3.5wt% nickel.

[0087] Impregnation: The catalyst carrier is placed in the impregnation solution and impregnated in a rotary evaporator at an equal volume for 60 minutes at 75-85°C. The impregnated carrier is placed in a watch glass and dried in a vacuum oven: first maintained at 80°C for 3 hours, then immediately heated to 120°C and maintained for 12 hours; then the dried sample is immediately placed in a muffle furnace for calcination: heated to about 800°C in an air atmosphere and maintained for 7 hours, then naturally cooled to room temperature to obtain a propane dehydrogenation catalyst.

[0088] Example 7

[0089] This embodiment provides a method for preparing a propane dehydrogenation catalyst using ACC wood preservative wastewater, which specifically includes the following steps:

[0090] Pretreatment: At room temperature, the ACC wood preservative wastewater was allowed to settle, and then the supernatant was filtered. The obtained filtrate was concentrated at normal pressure and 75-85°C to a saturated solution at 80°C. Then, the pH value was tested using an acidic pH test paper, and concentrated nitric acid was slowly added to adjust the pH of the saturated solution to ≤1 to obtain an impregnation solution.

[0091] Support: The zirconium oxide was immersed in a 0.08 mol / ml nickel nitrate aqueous solution, then maintained at 80°C for 3 hours, then maintained at 120°C for 12 hours for aging, and finally sintered at 700°C for 5 hours. The nickel content was detected to be 3wt%, thus obtaining a zirconium oxide support containing 3wt% nickel.

[0092] Impregnation: The catalyst carrier is placed in the impregnation solution and impregnated in a rotary evaporator at an equal volume for 40 minutes at 75-85°C. The impregnated carrier is placed in a watch glass and dried in a vacuum oven: first maintained at 80°C for 3 hours, then immediately heated to 120°C and maintained for 12 hours; then the dried sample is immediately placed in a muffle furnace for calcination: heated to about 700°C in a hydrogen atmosphere and maintained for 7 hours, then naturally cooled to room temperature to obtain a propane dehydrogenation catalyst.

[0093] Experimental example

[0094] The catalysts prepared in the examples and comparative examples were tableted and sieved to obtain particles of 20 to 40 mesh, which were then loaded into a 10 mL fixed bed stainless steel fixed bed reactor at a propane volume space velocity of 2 h -1 The reaction temperature was 600°C and propane was dehydrogenated to produce propylene at normal pressure. The specific 1-hour sampling catalyst evaluation results are shown in the following table.

[0095] The catalysts prepared in each embodiment and comparative example were tested for compressive strength according to the American Society for Testing and Materials ASTM D4179-11 (2017) standard, and the specific results are shown in the table below.

[0096] Table 1

[0097]

[0098]

[0099] It can be seen from the data in the above table that the conversion rate, selectivity, yield and mechanical strength of the propane dehydrogenation catalyst prepared by the method for preparing a propane dehydrogenation catalyst using ACC wood preservative wastewater provided by the present invention are basically close to the catalytic activity of the commercially available Cr dehydrogenation catalyst, and the cost is low. At the same time, the heavy metal ions in the ACC wood preservative wastewater are reused for a second time.

[0100] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the present invention, but these corresponding changes and deformations should all fall within the scope of protection of the claims of the present invention.

Claims

1. A method for preparing propane dehydrogenation catalyst using ACC wood preservative wastewater, characterized in that: The steps include: Pretreatment: After the ACC wood preservative wastewater is precipitated, the supernatant is filtered to remove impurities, and then concentrated to a saturated solution at normal pressure and 75-85°C, and the pH is adjusted to ≤1 to obtain an impregnation solution; Impregnation: adding the carrier to the impregnation solution for impregnation under stirring at 75-85° C., drying and calcining the impregnated carrier to obtain a propane dehydrogenation catalyst; Wherein, the carrier is a composite porous material formed by an inorganic porous material and a pore-forming agent, or an inorganic porous material containing 3wt% to 4wt% nickel.

2. The method according to claim 1, characterized in that In the pretreatment step, the calcination atmosphere is air, hydrogen or nitrogen.

3. The method according to claim 1, characterized in that The immersion is carried out in a rotary evaporator; preferably, the immersion time is 30 to 60 minutes.

4. The method according to claim 1, characterized in that The inorganic porous material is selected from at least one of macroporous alumina, high-purity alumina, mesoporous silica, zinc oxide, zirconium oxide, boron nitride and pseudo-boehmite.

5. The method according to claim 1, characterized in that The composite porous material is prepared by wet mixing an inorganic porous material and a pore-forming agent. Preferably, the mass ratio of the inorganic porous material to the pore-forming agent is 2 to 5:

1.

6. The method according to claim 1, characterized in that The inorganic porous material containing 3wt% to 4wt% nickel is obtained by immersing the inorganic porous material in a nickel nitrate solution, and then aging and sintering at 700 to 750°C for 5 to 6 hours.

7. The method according to claim 6, characterized in that The aging procedure is: first maintain at 80-90°C for 3-4 hours, then maintain at 120-140°C for 4-12 hours; and / or The concentration of the nickel nitrate is 0.001 mol / ml to 0.01 mol / ml.

8. The method according to claim 1, characterized in that In the pretreatment step, concentrated nitric acid is used to adjust the pH of the saturated solution.

9. The method according to claim 1, characterized in that The drying is vacuum drying, first drying at 75-85° C. for 3-4 hours, and then drying at 120-140° C. for 12-14 hours.

10. The method according to claim 1, characterized in that The calcination temperature is 650-850° C. and the calcination time is 7-10 hours.

Citation Information

Patent Citations

  • Dehydrogenation catalyst and preparation method and application thereof

    CN103769156A

  • Low-carbon alkane dehydrogenation microsphere catalyst preparation method

    CN107486197A

  • Propane dehydrogenation catalyst and preparation method thereof

    CN108654596A

  • Preparation method of chromium-based catalyst for preparation of propylene through propane dehydrogenation

    CN110841709A

  • Catalyst, method of manufacturing the same, and electrode catalyst

    JP2004113848A