Beneficiation process method for high-silicon copper oxide ore
Through multiple stirring treatment and adding specific agents, the high-silicon copper oxide ore ore ore dressing process method is solved, the problem of low recovery of copper oxide ore ore is improved, and the process flow is simplified.
Patent Information
- Application Number
- CN202411211233.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-03
AI Technical Summary
Due to its special properties, copper oxide ore has complex ore processing technology and low recovery rate, which limits the comprehensive utilization of copper oxide resources and the burden on enterprises.
A high-silicon oxide copper ore ore ore treatment is adopted, including grinding after crushing, multiple stirring treatments, adding sulfuric acid, sodium sulfide, sodium hydroxide and flocculant, and finally adding collector and foaming agent for flotation. , improve the recovery rate of copper oxide.
It significantly improves the recovery rate of copper oxide and the quality of copper concentrate, simplifies the flotation process, and reduces process complexity and environmental pressure.
Smart Images

Figure CN119056574A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of copper oxide ore dressing, and in particular to a high-silicon copper oxide ore dressing process method. Background Art
[0002] Oxidized copper ore has always been a difficult problem in the copper ore dressing industry. Due to its special properties, such as high mud content and poor floatability, the recovery rate of oxidized copper ore is low. Currently, the commonly used methods are physical beneficiation (sulfide flotation, oxidation flotation, etc.) and chemical beneficiation (acid leaching, ammonia leaching, etc.). These methods often have problems such as complex processes, low recovery rates, and high environmental pressure. Some mines can only carry out stockpiling treatment because the ore is extremely difficult to be sorted, which seriously restricts the comprehensive utilization of oxidized copper resources. At the same time, it also forms a heavy burden on enterprises. Summary of the invention
[0003] The present invention provides a high-silicon copper oxide ore beneficiation process method, which overcomes the shortcomings of the above-mentioned prior art and can effectively solve the problem of low copper oxide recovery rate due to the complex existing copper oxide ore beneficiation process.
[0004] In order to solve the above problems, a high-silicon copper oxide ore dressing process according to the present invention comprises the following steps: S1, grinding the copper oxide ore after crushing it to produce raw ore pulp; S2, adding sulfuric acid to the raw ore pulp in step S1 to perform a first stirring operation to produce a stirred ore pulp; S3, adding sodium sulfide to the slurry stirred in step S2 and performing a second stirring operation to produce a slurry with an acidic pH; S4, first adding sodium hydroxide to the ore pulp with an acidic pH in step S3, and then adding a flocculant to perform a third stirring operation, thereby producing an ore pulp after three stirrings; S5, after adding a collector and a frother to the ore pulp after three stirrings produced in step S4, a flotation operation is performed to produce a final copper concentrate and tailings.
[0005] In the above step S1, the copper oxide ore is crushed and then ground, including adding chalcocite or CuS mineral to the copper oxide ore, wherein the amount of chalcocite or CuS mineral added is 0.5%-1% of the weight of the original copper oxide ore, and the fineness is below -200 mesh, and the grinding operation is performed; wherein the grinding fineness is -200 mesh 60%-90%, and the mass concentration of the output raw ore slurry is 30%-40%.
[0006] The first stirring operation includes adding 2-5 kg / t of sulfuric acid based on the weight of the raw ore to the raw ore slurry for the first stirring operation, maintaining the pH of the output stirred slurry between 4-5, the stirring time is 10-20 minutes, and the stirring intensity is 200-600 r / min.
[0007] The second stirring operation includes adding 1-3 kg / t of sodium sulfide and then performing a second stirring operation to keep the pH of the slurry acidic, and the stirring time is 5 min to 10 min.
[0008] The third stirring operation includes first adding sodium hydroxide to adjust the pH to 9-10, and then adding 1-3g / t of flocculant for the third stirring operation, with a stirring time of 3-5min and a stirring intensity of 500-1000r / min.
[0009] The flocculant is polyacrylamide-glyoxal dihydroxyaniline.
[0010] The above-mentioned collector includes isopentyl xanthate, and the foaming agent includes 2# oil and MIBC.
[0011] The present invention can achieve the purpose of treating copper oxide ore by flotation by adding three stirring pretreatment operations before the flotation operation. Compared with the conventional flotation process, the method of the present invention can greatly improve the recovery rate of copper oxide and the quality of copper concentrate, and the flotation process is basically equivalent, and the process configuration is simpler. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] The specific implementation modes of the present invention will be further described in detail below in conjunction with the accompanying drawings.
[0013] Figure 1 This is a process flow chart of Example 1 of the present invention. DETAILED DESCRIPTION
[0014] The present invention is not limited by the following embodiments, and specific implementation methods can be determined based on the technical solution of the present invention and actual conditions.
[0015] Example 1: Figure 1 As shown, the embodiment of the present invention discloses a high-silicon copper oxide ore beneficiation process, comprising the following steps: S1, grinding the copper oxide ore after crushing it to produce raw ore pulp; S2, adding sulfuric acid to the raw ore pulp in step S1 to perform a first stirring operation to produce a stirred ore pulp; S3, adding sodium sulfide to the slurry stirred in step S2 and performing a second stirring operation to produce a slurry with an acidic pH; S4, first adding sodium hydroxide to the ore pulp with an acidic pH in step S3, and then adding a flocculant to perform a third stirring operation, thereby producing an ore pulp after three stirrings; S5, after adding a collector and a frother to the ore pulp after three stirrings produced in step S4, a flotation operation is performed to produce a final copper concentrate and tailings.
[0016] Wherein, in step S1, the copper oxide ore is crushed and then subjected to grinding operation, including, after adding chalcocite or CuS mineral to the copper oxide ore, the amount of chalcocite or CuS mineral added is 0.5%-1% of the weight of the original copper oxide ore, and the fineness thereof is below -200 mesh, and grinding operation is performed; wherein, the grinding fineness is -200 mesh 60%-90%, and the mass concentration of the output original ore slurry is 30%-40%.
[0017] The first stirring operation includes adding 2-5 kg / t of sulfuric acid based on the weight of the original ore to the original ore slurry for the first stirring operation, maintaining the pH of the output stirred slurry between 4-5, the stirring time is 10-20 minutes, and the stirring intensity is 200-600 r / min.
[0018] Among them, the second stirring operation includes adding 1-3kg / t of sodium sulfide and then performing the second stirring operation to keep the pH of the slurry acidic, and the stirring time is 5min-10min.
[0019] Among them, the third stirring operation includes first adding sodium hydroxide to adjust the pH to 9-10, and then adding 1-3g / t of flocculant for the third stirring operation. The stirring time is 3-5min and the stirring intensity is 500-1000r / min.
[0020] Among them, the collector includes advanced xanthate such as isopentyl xanthate, and the frother includes conventional flotation agents such as 2# oil and MIBC.
[0021] The present invention can achieve the purpose of treating copper oxide ore by flotation by adding three stirring pretreatment operations before the flotation operation. Compared with the conventional flotation process, the method of the present invention can greatly improve the recovery rate of copper oxide and the quality of copper concentrate, and the flotation process is basically equivalent, and the process configuration is simpler.
[0022] Embodiment 2: The embodiment of the present invention discloses a high-silicon copper oxide ore dressing process, comprising the following steps: (1) The ore is crushed and mixed, and 1 kg of copper oxide ore is added with 5 g of chalcocite, and then the ore is ground. The grinding fineness is -200 mesh 70%, and the slurry concentration is 35%.
[0023] (2) The slurry from step (1) was stirred for the first time by adding 2 kg / t of sulfuric acid based on the weight of the original ore. The pH of the slurry was 5, the stirring time was 20 min, and the stirring intensity was 200 r / min.
[0024] (3) After adding 1 kg / t sodium sulfide to the slurry stirred in step (2), a second stirring operation was performed to maintain the pH of the slurry at an acidic level for 5 min.
[0025] (4) To the slurry stirred in step (3), first add 2 kg / t sodium hydroxide to adjust the pH to 9, then add 1 g / t flocculant to perform a third stirring operation, with a stirring time of 3 min and a stirring intensity of 500 r / min.
[0026] (5) After adding 300 g / t of isopentyl xanthate and 50 g / t of 2# oil to the slurry stirred in step (4), conventional flotation operation is carried out. The operation process is "one roughing, two fine flotation, and two sweeping flotation", and the final copper concentrate and tailings can be produced.
[0027] In this embodiment, when the Cu grade of the original ore is 0.82%, a copper concentrate with a Cu grade of 18.56% and a recovery rate of 85.78% can be obtained.
[0028] Embodiment 3: The embodiment of the present invention discloses a high-silicon copper oxide ore dressing process, comprising the following steps: (1) The ore is crushed and mixed, 1 kg of copper oxide ore is added with 10 g of CuS, and then the ore is ground. The grinding fineness is -200 mesh 90%, and the ore pulp concentration is 40%.
[0029] (2) The slurry from step (1) was stirred for the first time by adding 5 kg / t of sulfuric acid based on the weight of the original ore. The pH of the slurry was 4, the stirring time was 10 min, and the stirring intensity was 600 r / min.
[0030] (3) After adding 3 kg / t sodium sulfide to the slurry stirred in step (2), a second stirring operation was performed to maintain the pH of the slurry at an acidic level for 5 min.
[0031] (4) To the slurry stirred in step (3), first add 3 kg / t sodium hydroxide to adjust the pH to 10, then add 3 g / t flocculant to perform a third stirring operation, the stirring time is 5 min, and the stirring intensity is 1000 r / min.
[0032] (5) After adding 400 g / t of isopentyl xanthate and 40 g / t of 2# oil to the slurry stirred in step (4), conventional flotation operation is carried out. The operation process is "one roughing, three fine flotation and two sweeping flotation", and copper concentrate and tailings can be finally produced.
[0033] In this embodiment, when the Cu grade of the original ore is 0.68%, a copper concentrate with a Cu grade of 22.34% and a recovery rate of 73.67% can be obtained.
[0034] Embodiment 4: The embodiment of the present invention discloses a high-silicon copper oxide ore dressing process, comprising the following steps: (1) The ore is crushed and mixed, and 1 kg of copper oxide ore is added with 10 g of chalcocite, and then the ore is ground. The grinding fineness is -200 mesh 80%, and the ore pulp concentration is 30%.
[0035] (2) The slurry from step (1) was stirred for the first time by adding 3 kg / t of sulfuric acid based on the weight of the original ore. The pH of the slurry was 4.5, the stirring time was 15 min, and the stirring intensity was 400 r / min.
[0036] (3) After adding 1.5 kg / t sodium sulfide to the slurry stirred in step (2), a second stirring operation was performed to maintain the pH of the slurry at an acidic level for 8 min.
[0037] (4) To the slurry stirred in step (3), 2 kg / t sodium hydroxide was first added to adjust the pH to 9.5, and then 2 g / t flocculant was added to perform a third stirring operation, with a stirring time of 4 min and a stirring intensity of 800 r / min.
[0038] (5) After adding 200 g / t of isopentyl xanthate and 30 g / t of 2# oil to the slurry stirred in step (4), conventional flotation operation is carried out. The operation process is "one roughing, two concentrating, and two sweeping", and copper concentrate and tailings can be finally produced.
[0039] In this embodiment, when the Cu grade of the original ore is 1.68%, a copper concentrate with a Cu grade of 25.83% and a recovery rate of 88.32% can be obtained.
[0040] Embodiment 5: The present invention proposes a high-silicon copper oxide ore dressing process, comprising the following steps: (1) The ore is crushed and mixed, and 1 kg of copper oxide ore is added with 5 g of CuS, and then the ore is ground. The grinding fineness is -200 mesh 85%, and the ore pulp concentration is 38%.
[0041] (2) The slurry from step (1) was stirred for the first time by adding 4 kg / t of sulfuric acid based on the weight of the original ore. The pH of the slurry was 4, the stirring time was 17 min, and the stirring intensity was 300 r / min.
[0042] (3) After adding 2 kg / t sodium sulfide to the slurry stirred in step (2), a second stirring operation was performed to maintain the pH of the slurry at an acidic level for 6 min.
[0043] (4) To the slurry stirred in step (3), 3 kg / t sodium hydroxide was first added to adjust the pH to 10, and then 1.5 g / t flocculant was added to perform a third stirring operation, with a stirring time of 4.5 min and a stirring intensity of 700 r / min.
[0044] (5) After adding 500 g / t of isopentyl xanthate and 35 g / t of 2# oil to the slurry stirred in step (4), conventional flotation operation is carried out. The operation process is "one roughing, two concentrating, and two sweeping", and copper concentrate and tailings can be finally produced.
[0045] In this example, when the Cu grade of the original ore is 2.83%, a copper concentrate with a Cu grade of 28.64% and a recovery rate of 83.25% can be obtained.
[0046] Embodiment 6: The embodiment of the present invention discloses a high-silicon copper oxide ore dressing process, comprising the following steps: (1) The ore is crushed and mixed, 1 kg of copper oxide ore is added with 8 g of CuS, and then the ore is ground. The grinding fineness is -200 mesh 60%, and the slurry concentration is 33%.
[0047] (2) The slurry from step (1) was stirred for the first time by adding 2.5 kg / t of sulfuric acid based on the weight of the original ore. The pH of the slurry was 4.3, the stirring time was 14 min, and the stirring intensity was 500 r / min.
[0048] (3) After adding 1.2 kg / t sodium sulfide to the slurry stirred in step (2), a second stirring operation was performed to maintain the pH of the slurry at an acidic level for 7 minutes.
[0049] (4) To the slurry stirred in step (3), 2.5 kg / t sodium hydroxide was first added to adjust the pH to 9.4, and then 2.5 g / t flocculant was added to perform a third stirring operation, with a stirring time of 3.5 min and a stirring intensity of 600 r / min.
[0050] (5) After adding 350 g / t of isopentyl xanthate and 60 g / t of 2# oil to the slurry stirred in step (4), conventional flotation operation is carried out. The operation process is "one roughing, three fine flotations and two sweeping flotations", and copper concentrate and tailings can be finally produced.
[0051] In this example, when the Cu grade of the original ore is 0.57%, a copper concentrate with a Cu grade of 17.33% and a recovery rate of 68.48% can be obtained.
Claims
1. A high silicon copper oxide ore dressing process, characterized in that: The following steps are involved: S1, grinding the copper oxide ore after crushing it to produce raw ore pulp; S2, adding sulfuric acid to the raw ore pulp in step S1 to perform a first stirring operation to produce a stirred ore pulp; S3, adding sodium sulfide to the slurry stirred in step S2 and performing a second stirring operation to produce a slurry with an acidic pH; S4, first adding sodium hydroxide to the ore pulp with an acidic pH in step S3, and then adding a flocculant to perform a third stirring operation, thereby producing an ore pulp after three stirrings; S5, after adding a collector and a frother to the ore pulp after three stirrings produced in step S4, a flotation operation is performed to produce a final copper concentrate and tailings.
2. A high silicon copper oxide ore dressing process according to claim 1, characterized in that: In the step S1, the copper oxide ore is crushed and then subjected to grinding operation, including adding chalcocite or CuS mineral to the copper oxide ore, wherein the amount of chalcocite or CuS mineral added is 0.5%-1% of the weight of the original copper oxide ore, and the fineness thereof is below -200 mesh, and then grinding operation is performed; wherein the grinding fineness is -200 mesh 60%-90%, and the mass concentration of the output raw ore pulp is 30%-40%.
3. The high silicon copper oxide ore dressing process according to claim 1, characterized in that: The first stirring operation includes adding 2-5 kg / t of sulfuric acid based on the weight of the original ore to the original ore pulp for the first stirring operation, maintaining the pH of the output stirred pulp between 4-5, the stirring time is 10-20 minutes, and the stirring intensity is 200-600 r / min.
4. The high silicon copper oxide ore dressing process according to claim 1, characterized in that: The second stirring operation includes adding 1-3 kg / t of sodium sulfide and then performing a second stirring operation, keeping the pH of the slurry acidic, and the stirring time is 5 min-10 min.
5. The high silicon copper oxide ore dressing process according to claim 1, characterized in that: The third stirring operation includes first adding sodium hydroxide to adjust the pH to 9-10, and then adding 1-3g / t of flocculant for the third stirring operation, the stirring time is 3-5min, and the stirring intensity is 500-1000r / min.
6. The high silicon copper oxide ore dressing process according to claim 1, characterized in that: The flocculant is polyacrylamide-glyoxal dihydroxyaniline.
7. The high silicon copper oxide ore dressing process according to claim 1, characterized in that: The collector includes isopentyl xanthate, and the foaming agent includes 2# oil and MIBC.
Citation Information
Patent Citations
Beneficiation method for copper-gold tailings with complex sources
CN113908973A
Process method for copper oxide beneficiation by adopting hydrogen sulfide
CN117225599A
Combined regulator and process method for beneficiation of copper oxide ore by adopting combined regulator
CN117358429A
Branch carrier floatation and agitating tank with perforated baffle