TiNN-MFP5 composite coating for medical titanium product and preparation method of TiNN-MFP5 composite coating

Through the hydrogen bonding of NaOH alkali heat treatment and mussel protein, the TiNN-MFP5 composite coating was prepared, which solved the problem of medical titanium materials being susceptible to microbial contamination in the human body, significantly improved antibacterial performance and biocompatibility, and extended use Lifespan and promotes tissue healing.

CN119056724APending Publication Date: 2024-12-03SHANGHAI UNIV OF ENG SCI +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411187769.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Medical titanium materials are susceptible to microbial contamination in the human body, resulting in poor implant integration, inflammation, mechanical instability, necrosis and infection complications, and lack the function to promote tissue regeneration and repair, making it difficult to closely combine with skin soft tissues and increase bacteria. Invasion and inflammation risks.

Method used

NaOH alkaline heat treatment is used to form a nanonetwork structure and a TiO2 passivation membrane, and the Dopa of mussel protein combines to form hydrogen bonds with the TiO2 surface to prepare a TiNN-MFP5 composite coating to enhance antibacterial performance and cell adhesion ability.

Benefits of technology

It significantly improves the antibacterial properties and biocompatibility of titanium-based materials, reduces bacterial infection and tissue rejection, extends the service life of the implant, and promotes tissue healing and cell growth.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119056724A_ABST
    Figure CN119056724A_ABST
Patent Text Reader

Abstract

The invention discloses a TiNN-MFP5 composite coating for a medical titanium product and a preparation method of the TiNN-MFP5 composite coating, and the preparation method comprises the following steps: pre-treating the medical titanium product, including grinding, polishing, cleaning and sterilizing; performing alkali heat treatment to form a nano network structure on the surface of the medical titanium product; performing high-temperature sterilization on the treated titanium product; the sterilized titanium product is soaked in an MFP-5 solution to form an MFP5 coating, and the obtained titanium product is covered with a TiNN-MFP5 composite coating. A nano-network structure is formed on the surface of the titanium product for traditional Chinese medicine, and mussel protein containing Dopa covers the nano-network structure, so that the adhesion capacity of cells is remarkably improved, and rapid fusion and healing of an implant and surrounding tissues are promoted. Meanwhile, the coating has an excellent antibacterial property, effectively inhibits the breeding of germs on the surface of the implant, reduces the infection risk, and can be widely applied to titanium-based medical implants such as bone fixing instruments, joint prostheses and dental implants.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of biomedical materials, and specifically relates to a TiNN-MFP5 composite coating for medical titanium products and a preparation method thereof. Background Art

[0002] Titanium and its alloys are widely used in biomedical materials due to their superior properties, including low density (4.5g / cm 3 ), non-magnetic, low elastic modulus, corrosion resistance, non-toxicity and high strength. In addition, the elastic modulus of titanium is close to that of human bone, showing good biocompatibility, providing a solid foundation and broad prospects for its application in the biomedical field. In orthopedic surgery, titanium is often used to make supporting and replacement materials, such as screws, plates, nails and implants of artificial joints; in medical devices, titanium is used as a raw material for scalpels, scissors and stents; in addition, titanium is also an ideal choice for oral restoration materials such as dental implants. However, due to the large number of microbial communities inside and outside the human body, including bacteria, viruses, fungi and other microorganisms, medical titanium materials are easily contaminated. As a metal implant, titanium may cause complications such as poor implant integration, inflammation, mechanical instability, necrosis and infection when implanted into the human body, which seriously threatens the health of patients. In addition, titanium itself does not have the function of promoting tissue regeneration and repair, which makes it difficult to closely integrate with skin soft tissue when used as a percutaneous implant, thereby increasing the risk of bacterial invasion and inflammation around the implant. Therefore, improving the antibacterial properties and cell adhesion ability of titanium implants has become a research hotspot.

[0003] Studies have found that titanium-based surface modification is an effective method to improve its performance, including non-coating surface treatment and coating surface treatment. Among them, the mechanical method is the most basic and simplest method in the non-coating method, which can directly change the original structure or chemical composition of the material surface, and is usually used in combination with other modification methods. In addition, researchers tend to combine non-coating and coating methods to achieve the best effects of both. Combining mechanical methods with other surface modification techniques (such as chemical treatment or heat treatment) can significantly improve the biocompatibility and surface properties of titanium-based materials. At the same time, combined with coating technology (such as protein coating), the antibacterial properties and cell adhesion ability of titanium-based materials are further enhanced. This composite treatment method can not only improve the initial surface properties of the implant, but also maintain its excellent biocompatibility and antibacterial properties during long-term use, thereby reducing the risk of postoperative infection, promoting tissue healing, and extending the service life and safety of the implant.

[0004] Mussel adhesive protein (MAP) is considered to be an ideal surface protein coating material due to its excellent adhesion properties and biocompatibility. It is well known that mussels adhere to the surface of the ocean by secreting adhesive proteins. The solid patches formed by these proteins can firmly adhere to various wet surfaces such as rocks, metals, polymers and wooden structures. The adhesion of mussel adhesive proteins is closely related to the presence of 3,4-dihydroxyphenylalanine (DOPA), a catechol amino acid formed by post-translational modification of tyrosine. DOPA can adhere to different types of substrates through a variety of chemical bonds (including hydrogen bonds, metal-catechol coordination bonds, π-π / π-cation interactions, oxidative cross-linking and electrostatic interactions). Among them, MFP-5 is considered to be the main adhesive protein with a high DOPA content, and it exhibits high biocompatibility and biodegradability and does not induce immune response. Studies have shown that mussel proteins increase cell adsorption on the surface of substrates and can effectively prevent bacterial invasion. At present, there are no reports on the use of hydrogen bonds between mussel proteins and TiO2 to adhere to the surface of biomedical products to obtain composite coatings. Summary of the invention

[0005] Based on this, the main purpose of the present invention is to provide a method for preparing a TiNN-MFP5 composite coating for medical titanium products, which forms a nano-network structure and a thicker TiO2 passivation film after NaOH alkaline heat treatment, and then utilizes the hydrogen bonds formed between Dopa of mussel protein and TiO2 to make it adhere to the surface of medical titanium products to obtain a TiNN-MFP5 composite coating. The preparation method is simple and easy, and has high operability and wide applicability.

[0006] Another object of the present invention is to provide a TiNN-MFP5 composite coating obtained by the above-mentioned preparation method. The composite coating not only has the corrosion resistance, biostability and excellent cell growth promotion properties of the TiNN coating, but also has the antibacterial and cell-promoting activity of the mussel protein coating. It can effectively reduce the complications caused by medical titanium products in clinical practice, such as bacterial infection and tissue rejection reaction, thereby extending the service life and improving the medical effect.

[0007] To achieve the above object, the present invention adopts the following technical solution:

[0008] The present invention provides a method for preparing a TiNN-MFP5 composite coating for medical titanium products, comprising the following steps:

[0009] (1) Medical titanium products (TA1) were polished with silicon carbide water-abrasive sandpaper until the surface scratches were uniform, and then polished with silicon dioxide polishing liquid;

[0010] (2) The polished TA1 was ultrasonically cleaned with acetone, anhydrous ethanol and deionized water for 20-30 min in sequence, dried at 60-80°C, and sterilized at high temperature;

[0011] (3) After cleaning and sterilization, TA1 is immersed in a constant temperature water bath at 50-70°C and a concentration of 4-6M sodium hydroxide solution for 18-30 hours. Then, it is taken out and rinsed with ultrapure water until the conductivity of the rinse solution is less than 5uS / cm 3 , obtaining a medical titanium product with a nano-network structure (TiNN);

[0012] (4) After the TiNN is allowed to dry, it is sterilized at high temperature;

[0013] (5) Filter the recombinant mussel adhesion protein type 5 (MFP-5) solution using a 0.22 μm sterile syringe filter in a biological safety cabinet to remove impurities and microorganisms;

[0014] (6) Using the immersion coating method, the TiNN was immersed in the MFP-5 solution in a biological safety cabinet and allowed to stand overnight at 4° C. to form a mussel protein coating (MFP5) on its surface. After the coating was formed, it was gently rinsed in deionized water and dried to obtain a TiNN-MFP5 composite coating.

[0015] Preferably, in step (1), a silicon dioxide polishing liquid is used for polishing to an accuracy of 0.04 um.

[0016] Preferably, in step (1), the medical titanium product is a medical pure titanium disc with a diameter of 12 mm and a thickness of 3 mm, which is first polished in sequence with 240 mesh, 400 mesh, 600 mesh, 800 mesh, 1000 mesh, 1200 mesh, 1500 mesh, and 2000 mesh silicon carbide water-abrasive paper under running water of a metallographic grinder and polisher until the surface scratches are consistent, and then polished with W3, W1, W0.5, W0.05, and W0.02 silicon dioxide polishing liquids.

[0017] Preferably, in step (3), the temperature of the constant temperature water bath is maintained at 60° C., the constant temperature water bath time is 24 h, and the concentration of the sodium hydroxide solution is 5 M.

[0018] Preferably, in step (5), the concentration of the MFP-5 solution is 0.5 to 10 mg / mL.

[0019] Preferably, in step (6), the overnight standing time at 4°C is not less than 12 hours, and the drying temperature is 20-30°C.

[0020] The present invention also provides a TiNN-MFP5 composite coating for medical titanium products, which is obtained by the preparation method of the aforementioned TiNN-MFP5 composite coating, and comprises a TiNN coating and a mussel protein coating sequentially covering the surface of the medical titanium product, and the TiNN coating has a nano-network structure.

[0021] The present invention also provides the use of the TiNN-MFP5 composite coating in preparing titanium-based medical implants with antibacterial and cell-promoting activities.

[0022] The present invention also provides a titanium-based medical implant, which comprises the aforementioned TiNN-MFP5 composite coating.

[0023] Preferably, the titanium-based medical implants include bone fixation instruments, joint prostheses and dental implants.

[0024] In the present invention, first, a TiNN coating with a nano-network structure is formed on the titanium surface by NaOH alkali heat treatment. This structure not only significantly increases the surface area, but also helps the attachment and growth of cells, and improves the biocompatibility of titanium-based materials. In addition, NaOH alkali heat treatment also forms a thicker TiO2 passivation film, which further improves the corrosion resistance and biostability of the material. Next, the treated titanium sheet is immersed in a mussel protein solution containing Dopa. The Dopa molecules form a strong adhesion with the TiO2 surface through hydrogen bonds, so that the mussel protein is evenly covered on the titanium surface to form a second coating. The mussel protein coating not only has excellent antibacterial properties, but also can significantly promote cell adhesion and proliferation.

[0025] The TiNN-MFP5 composite coating obtained by the aforementioned preparation method of the present invention combines the dual advantages of the TiNN coating and the mussel protein coating. The TiNN coating provides a good cell growth environment and enhances the biocompatibility of the material. The mussel protein coating gives the material excellent antibacterial properties and the ability to promote cell adhesion. This composite coating can effectively reduce the complications caused by medical titanium products in clinical applications, such as bacterial infection and tissue rejection, thereby extending their service life and improving medical effects. In addition, the preparation method of the present invention is simple and easy, and has high operability and wide applicability. By optimizing the process parameters, the TiNN-MFP5 composite coating can be uniformly formed on medical titanium-based materials of different shapes and sizes. It is not only suitable for common medical titanium products such as bone fixation instruments, joint prostheses and dental implants, but can also be applied to other biomedical materials that require surface modification, providing new technical paths and application prospects for the development of the field of biomaterials.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] 1) Significantly improve antibacterial properties: The mussel protein contained in the TiNN-MFP5 composite coating has excellent antibacterial properties. Its strong positive charge can interact with the negative charge on the bacterial surface, destroy the cell membrane structure, and effectively inhibit the growth of bacteria on the surface of medical titanium products, thereby reducing the risk of postoperative infection, which is of great significance to the safety of implants and the postoperative recovery of patients.

[0028] 2) Promote cell adhesion and growth: The nano-network structure of the TiNN coating and the mussel protein coating work together to significantly improve the cell adhesion and growth ability of titanium-based materials. In addition, the TiNN coating provides a suitable microenvironment that is conducive to cell attachment and proliferation, and the mussel protein coating further enhances cell adhesion and accelerates tissue fusion and healing.

[0029] 3) Improve biocompatibility and stability: The TiNN-MFP5 composite coating combined with the excellent corrosion resistance and biocompatibility of the TiO2 passivation film can maintain long-term stability in the in vivo environment, helping to reduce complications caused by material degradation or corrosion and improve the service life and reliability of the implant. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 : (a) Schematic diagram of the scanning electron microscope (SEM) of the surface of the medical titanium product (TA1) without any treatment in Example 1; (b) Schematic diagram of the SEM of the surface of the medical titanium product (TiNN) after alkaline heat treatment with sodium hydroxide in Example 1; (c) Schematic diagram of the SEM of the surface of the medical titanium product (TiNN-MFP5) after alkaline heat treatment coated with MFP-5 protein solution in Example 1.

[0031] Figure 2 : Schematic diagram of EDS element content on the surfaces of TA1, TiNN and TiNN-MFP5 in Example 1, (a) is the atomic number percentage of the sample (Atomic Conc.); (b) is the mass percentage of the sample (Weight Conc).

[0032] Figure 3 : (a) Schematic diagram of atomic force microscopy (AFM) on the TA1 surface in Example 1; (b) Schematic diagram of AFM on the TiNN surface in Example 1; (c) Schematic diagram of AFM on the TiNN-MFP5 surface in Example 1.

[0033] Figure 4 : Schematic diagram of the surface contact angles and average contact angles of TA1, TiNN and TiNN-MFP5 in Example 1, (a) is the average contact angle, and (b) is the surface water contact angle.

[0034] Figure 5: Infrared absorption spectra (ATR-FTIR) of TA1, TiNN and TiNN-MFP5 in Example 1.

[0035] Figure 6 : The flat coating effect diagram of Gram-negative bacteria Escherichia coli (E. coli) and Gram-positive bacteria Staphylococcus aureus (S. aureus) in Example 1 after being cultured on the surface of each sample for 24 hours, reflecting the antibacterial performance, (a) E. coli; (b) S. aureus.

[0036] Figure 7 : The comparison chart of the cell activity of human fibroblasts on the surfaces of medical titanium products with different surface treatments in Example 1 reflects the promotion of cell adhesion and growth. DETAILED DESCRIPTION

[0037] In order to more fully understand and demonstrate the technical solutions, purposes and advantages of the present invention, the technical effects produced by the present invention are further described in detail and completely in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all. It should be pointed out that for those of ordinary skill in the art, other embodiments obtained without departing from the concept of the present invention all belong to the protection scope of the present invention, and the present invention is specifically described in conjunction with the accompanying drawings and embodiments.

[0038] Unless otherwise specified in the following examples, all reagents and materials used were commercially available.

[0039] Example 1

[0040] In this example, TA1 pure titanium was used as the matrix to prepare the TiNN-MFP5 composite coating. First, NaOH alkaline heat treatment was used to form a nano-network structure and a thicker TiO2 passivation film, and then MFP5 was immobilized on the pure titanium surface through the hydrogen bond formed between Dopa of mussel protein and TiO2, thus obtaining a TiNN-MFP5 composite coating with excellent antibacterial properties and cell adhesion ability.

[0041] Preparation steps

[0042] Using medical titanium product TA1 as the substrate, discs with a size of Φ12mm×3mm were cut out.

[0043] The process parameters for preparing TiNN-MFP5 composite coating are:

[0044] NaOH concentration, water bath heating temperature and time: 5 mol / L, 60°C, 24 h;

[0045] MFP-5 concentration: 5 mg / mL.

[0046] The method for preparing the above TiNN-MFP5 composite coating comprises the following steps:

[0047] (1) The medical titanium product TA1 was polished with 240 mesh, 400 mesh, 600 mesh, 800 mesh, 1000 mesh, 1200 mesh, 1500 mesh, and 2000 mesh silicon carbide water-abrasive paper in a metallographic polishing machine under running water until the surface scratches were consistent, and then polished with W3, W1, W0.5, W0.05, and W0.02 silicon dioxide polishing liquid in turn.

[0048] (2) The polished titanium product (TA1) was ultrasonically cleaned with acetone, anhydrous ethanol, and deionized water for 20-30 min, dried in a drying oven at 70°C, and then sterilized at high temperature.

[0049] (3) After cleaning and sterilization, the titanium product (TA1) was immersed in a 5M sodium hydroxide solution at 60°C in a constant temperature water bath (60°C) for 24 hours, then taken out and rinsed with ultrapure water until the conductivity of the rinse solution was less than 5uS / cm 3 , and obtain a titanium product with a nano-network structure (TiNN).

[0050] (4) The treated titanium product with a nano-network structure (TiNN) was left to dry and then sterilized at a high temperature of 121°C.

[0051] (5) The MFP-5 solution (5 mg / mL) was push-filtered using a 0.22 μm sterile syringe filter in a biosafety cabinet to remove impurities and microorganisms.

[0052] (6) Using the immersion coating method, the sterile titanium product with a nano-network structure (TiNN) was immersed in the MFP-5 solution in a biological safety cabinet, and then placed in a 4°C refrigerator and allowed to stand overnight to form a mussel protein coating (MFP5) on its surface. After the coating was formed, it was gently rinsed in deionized water and dried to obtain a TiNN-MFP5 composite coating.

[0053] Example 2

[0054] In this example, TA1 pure titanium was used as the matrix to prepare a TiNN-MFP5 composite coating. A nano-network structure and a thicker TiO2 passivation film were formed by NaOH alkaline heat treatment, and the mussel protein coating (MFP5) was fixed on the pure titanium surface through the hydrogen bond formed between Dopa of the mussel protein and TiO2, thereby obtaining a TiNN-MFP5 composite coating with excellent antibacterial properties and cell adhesion ability.

[0055] Preparation steps

[0056] Using medical titanium product TA1 as the substrate, a disc with a size of Φ12mm×3mm was cut;

[0057] The process parameters for preparing TiNN-MFP5 composite coating are:

[0058] NaOH concentration, water bath heating temperature and time: 5 mol / L, 60°C, 24 h;

[0059] MFP-5 concentration: 0.5 mg / mL.

[0060] The method for preparing the above TiNN-MFP5 composite coating comprises the following steps:

[0061] (1) The medical titanium product TA1 was polished with 240 mesh, 400 mesh, 600 mesh, 800 mesh, 1000 mesh, 1200 mesh, 1500 mesh, and 2000 mesh silicon carbide water-abrasive paper in a metallographic polishing machine under running water until the surface scratches were consistent, and then polished with W3, W1, W0.5, W0.05, and W0.02 silicon dioxide polishing liquid in turn.

[0062] (2) The polished titanium product (TA1) was ultrasonically cleaned with acetone, anhydrous ethanol, and deionized water for 20-30 min, dried in a drying oven at 70°C, and then sterilized at high temperature.

[0063] (3) After cleaning and sterilization, the titanium product (TA1) was immersed in a 5M sodium hydroxide solution at 60°C in a constant temperature water bath (60°C) for 24 hours, then taken out and rinsed with ultrapure water until the conductivity of the rinse solution was less than 5uS / cm 3 , and obtain a titanium product with a nano-network structure (TiNN).

[0064] (4) The treated titanium product with a nano-network structure (TiNN) was left to dry and then sterilized at a high temperature of 121°C.

[0065] (5) The MFP-5 solution (0.5 mg / mL) was push-filtered using a 0.22 μm sterile syringe filter in a biosafety cabinet to remove impurities and microorganisms.

[0066] (6) Using the immersion coating method, the sterile titanium product with a nano-network structure (TiNN) was immersed in the MFP-5 solution in a biological safety cabinet, and then placed in a 4°C refrigerator and allowed to stand overnight to form a mussel protein coating (MFP5) on its surface. After the coating was formed, it was gently rinsed in deionized water and dried to obtain a TiNN-MFP5 composite coating.

[0067] Example 3

[0068] In this example, TA1 pure titanium was used as the matrix to prepare a TiNN-MFP5 composite coating. A nano-network structure and a thicker TiO2 passivation film were formed by NaOH alkaline heat treatment, and the mussel protein coating (MFP5) was fixed on the pure titanium surface through the hydrogen bond formed between Dopa of mussel protein and TiO2, thereby preparing a TiNN-MFP5 composite coating with excellent antibacterial properties and cell adhesion ability.

[0069] Preparation steps

[0070] Using medical titanium product TA1 as the substrate, a disc with a size of Φ12mm×3mm was cut;

[0071] The process parameters of the prepared TiNN-MFP5 composite coating are:

[0072] NaOH concentration, water bath heating temperature and time: 5 mol / L, 60°C, 24 h;

[0073] MFP-5 concentration: 10 mg / mL.

[0074] The method for preparing the above TiNN-MFP5 composite coating comprises the following steps:

[0075] (1) The medical titanium product TA1 was polished with 240 mesh, 400 mesh, 600 mesh, 800 mesh, 1000 mesh, 1200 mesh, 1500 mesh, and 2000 mesh silicon carbide water-abrasive paper in a metallographic polishing machine under running water until the surface scratches were consistent, and then polished with W3, W1, W0.5, W0.05, and W0.02 silicon dioxide polishing liquid in turn.

[0076] (2) The polished titanium product (TA1) was ultrasonically cleaned with acetone, anhydrous ethanol, and deionized water for 20-30 min, dried in a drying oven at 70°C, and then sterilized at high temperature.

[0077] (3) After cleaning and sterilization, the titanium product (TA1) was immersed in a 5M sodium hydroxide solution at 60°C in a constant temperature water bath (60°C) for 24 hours, then taken out and rinsed with ultrapure water until the conductivity of the rinse solution was less than 5uS / cm 3 , and obtain a titanium product with a nano-network structure (TiNN).

[0078] (4) The treated titanium product with a nano-network structure (TiNN) was left to dry and then sterilized at a high temperature of 121°C.

[0079] (5) The MFP-5 solution (10 mg / mL) was push-filtered using a 0.22 μm sterile syringe filter in a biosafety cabinet to remove impurities and microorganisms.

[0080] (6) Using the immersion coating method, the sterile titanium product with a nano-network structure (TiNN) was immersed in the MFP-5 solution in a biological safety cabinet, and then placed in a 4°C refrigerator and allowed to stand overnight to form a mussel protein coating (MFP5) on its surface. After the coating was formed, it was gently rinsed in deionized water and dried to obtain a TiNN-MFP5 composite coating.

[0081] The characterization method and performance test results are as follows:

[0082] The samples were characterized by scanning electron microscopy (SEM) to confirm whether the coating was successfully applied, and energy dispersive X-ray spectroscopy (EDX) was used to analyze the main elemental composition of the coating, such as Figure 1 and 2 shown. Figure 1 The surface morphology of the TiNN-MFP5 composite coating (c) has changed significantly compared to the surface of the medical titanium product (a). The presence of a nano-network structure and a layer of film can be seen, proving that the coating has been successfully applied. Figure 2 Both (a) and (b) show that the oxygen (O) content of the medical titanium product (TiNN) after alkaline heat treatment with sodium hydroxide increased compared with the medical titanium product (TA1), and a small amount of sodium (Na) element appeared, proving that a layer of titanium dioxide (TiO2) protective film was formed on the surface after alkaline heat treatment. The medical titanium product (TiNN-MFP5) after alkaline heat treatment coated with MFP-5 protein solution showed a large amount of carbon element (C) compared with the medical titanium product (TiNN) after alkaline heat treatment with sodium hydroxide, proving the successful coating of MFP-5 (type 5 recombinant mussel adhesion protein).

[0083] Atomic force microscopy (AFM) was used to characterize the samples to obtain their three-dimensional surface morphology and surface roughness (Ra), such as Figure 3 Compared with the surface of medical titanium products (a), the surface of titanium metal (TiNN) after alkali heat treatment (b) is rougher, and the three-dimensional surface morphology can be seen to be very different from the surface of titanium products. Compared with (b) and (a), the surface morphology of (c) has changed again, the surface roughness has decreased, the surface is smoother, and the protein particles are spread more evenly.

[0084] The contact angle measurement instrument is used to characterize the hydrophilicity and hydrophobicity of the sample, such as Figure 4 Compared with the surface of medical titanium products and the titanium metal surface after heat treatment (TiNN), the water contact angle of the TiNN-MFP5 composite coating surface is the smallest and the hydrophilicity is the best. The presence of the coating improves the hydrophilicity of the surface.

[0085] Measure 400-4000cm using infrared spectrometer -1The attenuated reflection Fourier transform infrared spectrum in the range is used to obtain the infrared absorption spectrum, and the composition analysis of the sample is carried out to further verify the existence of the composite coating. Figure 5 As shown, the infrared absorption peak on the surface of the TiNN-MFP5 composite coating showed the characteristic absorption peak of Dopa and the characteristic absorption peak of TiO2, which further verified the successful coverage of the coating.

[0086] The antibacterial properties of the coating against E.coli and S.aureus were analyzed by plate coating method. Figure 6 As shown, the antibacterial effect of the TiNN-MFP5 composite coating surface is the best, and the antibacterial rate reaches 100% compared with TA1.

[0087] The cell viability of human fibroblasts on titanium surfaces treated with different methods was analyzed by cell culture. Figure 7 As shown, the TiNN-MFP5 composite coating surface is more conducive to the growth of human fibroblasts.

[0088] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a TiNN-MFP5 composite coating for medical titanium products, characterized in that: The following steps are involved: (1) Medical titanium products (TA1) were polished with silicon carbide water-abrasive sandpaper until the surface scratches were uniform, and then polished with silicon dioxide polishing liquid; (2) The polished TA1 was ultrasonically cleaned with acetone, anhydrous ethanol and deionized water for 20-30 min in sequence, dried at 60-80°C, and sterilized at high temperature; (3) After cleaning and sterilization, TA1 is immersed in a constant temperature water bath at 50-70°C and a concentration of 4-6M sodium hydroxide solution for 18-30 hours. Then, it is taken out and rinsed with ultrapure water until the conductivity of the rinse solution is less than 5uS / cm 3 , obtaining a medical titanium product with a nano-network structure (TiNN); (4) After the TiNN is allowed to dry, it is sterilized at high temperature; (5) Filter the recombinant mussel adhesion protein type 5 (MFP-5) solution using a 0.22 μm sterile syringe filter in a biological safety cabinet to remove impurities and microorganisms; (6) Using the immersion coating method, the TiNN was immersed in the MFP-5 solution in a biological safety cabinet and allowed to stand overnight at 4° C. to form a mussel protein coating (MFP5) on its surface. After the coating was formed, it was gently rinsed in deionized water and dried to obtain a TiNN-MFP5 composite coating.

2. The method for preparing the TiNN-MFP5 composite coating according to claim 1, characterized in that: In step (1), a silicon dioxide polishing liquid is used for polishing to an accuracy of 0.04 um.

3. The method for preparing the TiNN-MFP5 composite coating according to claim 1, characterized in that: In step (1), the medical titanium product is a medical pure titanium disc with a diameter of 12 mm and a thickness of 3 mm. It is first polished with 240 mesh, 400 mesh, 600 mesh, 800 mesh, 1000 mesh, 1200 mesh, 1500 mesh, and 2000 mesh silicon carbide water-abrasive paper in sequence under running water of a metallographic grinder and polisher until the surface scratches are consistent, and then polished with W3, W1, W0.5, W0.05, and W0.02 silicon dioxide polishing liquid.

4. The method for preparing the TiNN-MFP5 composite coating according to claim 1, characterized in that: In step (3), the temperature of the constant temperature water bath is maintained at 60° C., the constant temperature water bath time is 24 h, and the concentration of the sodium hydroxide solution is 5 M.

5. The method for preparing the TiNN-MFP5 composite coating according to claim 1, characterized in that: In step (5), the concentration of the MFP-5 solution is 0.5 to 10 mg / mL.

6. The method for preparing the TiNN-MFP5 composite coating according to claim 1, characterized in that: In step (6), the overnight standing time at 4°C is not less than 12 hours, and the drying temperature is 20-30°C.

7. A TiNN-MFP5 composite coating for medical titanium products, obtained by the preparation method of the TiNN-MFP5 composite coating according to any one of claims 1 to 6, comprising a TiNN coating and a mussel protein coating sequentially covering the surface of the medical titanium product, and the TiNN coating has a nano-network structure.

8. Use of the TiNN-MFP5 composite coating according to claim 7 in the preparation of titanium-based medical implants with antibacterial and cell-promoting activities.

9. A titanium-based medical implant, characterized in that: It comprises the TiNN-MFP5 composite coating as described in claim 7.

10. The titanium-based medical implant according to claim 9, characterized in that The titanium-based medical implants include bone fixation instruments, joint prostheses and dental implants.