Preparation method of titanium alloy sheet

By reasonably setting the deformation amount and heat treatment system of hot and cold rolling, combined with the surface treatment process, TB2 titanium alloy thin plates were prepared, which solved the problem of lack of systematic preparation technology in the existing technology and achieved mass production that meets the performance requirements of aviation structural materials.

CN119056871APending Publication Date: 2024-12-03JIANGSU XIANGYUN TITANIUM ALLOY NEW MATERIALS CO LTD

Patent Information

Application Number
CN202411350817.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-26
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing technology lacks a systematic TB2 titanium alloy thin plate preparation process, which is difficult to meet the needs of aviation structural materials, and has not formed a mass-producible preparation method.

Method used

By setting up a reasonable deformation and heat treatment system for hot and cold rolling, combined with the surface treatment process, it includes multiple heat-heating rolling, solid solution treatment, sand blasting and pickling to remove the oxide scale, cold rolling to the target thickness, and surface repair Grinding and finishing, a TB2 titanium alloy thin plate that meets the requirements of GB/T 3621 was prepared.

Benefits of technology

It has achieved good mechanical and technological performance of TB2 titanium alloy thin plates, met the performance requirements of aviation structural materials, and can be mass-produced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119056871A_ABST
    Figure CN119056871A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a titanium alloy sheet, and relates to the technical field of titanium alloys, the preparation method comprises the following steps: S1, heating and rolling a titanium alloy plate blank to obtain a first rolled plate blank; s2, the first rolled plate blank is subjected to fixed-length slitting and coping; s3, the first rolled plate blank is heated and rolled, and a second rolled plate blank is obtained; s4, the second rolled plate blank is ground; s5, the second rolled plate blank is heated and rolled to obtain a third rolled plate blank; step S6, solution treatment; s7, the third rolled plate blank is subjected to sand blasting treatment, acid pickling and coping; s8, the third rolled plate blank is subjected to cold rolling; s9, the plate blank is subjected to solution treatment; s10, the cold-rolled plate blank is subjected to alkali washing treatment and acid washing treatment; and S11, the plate blank is subjected to fixed-length slitting, and the titanium alloy thin plate is obtained. The titanium alloy plate prepared by reasonably setting the hot and cold rolling deformation, the heat treatment system and the surface treatment process is good in mechanical and technological performance and meets the GB / T 3621 technical requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of titanium alloys, and in particular relates to a method for preparing a titanium alloy thin plate. Background Art

[0002] TB2 (Ti-5Mo-5V-8Cr-3Al) alloy is a metastable β-type titanium alloy. This alloy has excellent cold forming properties, corrosion resistance, contact corrosion resistance and good welding properties in the solution treated state. It has high strength and good plasticity in the solution aging state. The main semi-finished products of TB2 include plates, strips, foils, bars, wires, etc. Plates can be made into sheet metal parts, pressure vessels, solid rocket engine casings, etc.

[0003] At present, although there is a certain research basis for the process, structure, and properties of TB2 titanium alloy, there is little systematic research on the preparation process of TB2 titanium alloy hot and cold rolled plates, and there is no relatively complete and mass-producible TB2 titanium alloy thin plate preparation process and technical support. Therefore, in order to meet the growing demand for aviation structural materials, it is very necessary to propose a preparation method for TB2 titanium alloy thin plates. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for preparing a titanium alloy thin plate. By reasonably setting the hot and cold rolling deformation, heat treatment system and surface treatment process, the TB2 titanium alloy plate prepared has good mechanical and process properties and meets the technical requirements of GB / T 3621. TB2 titanium alloy thin plates that meet the performance requirements can be mass-produced.

[0005] The technical solution adopted by the present invention is:

[0006] A method for preparing a titanium alloy thin plate, comprising the following steps:

[0007] Step S1. heating a titanium alloy slab with a thickness of 100 mm to 160 mm to T1 and keeping the temperature at t1, and then rolling it to a thickness of 10 mm to 20 mm in a hot rolling mill to obtain a first rolled slab;

[0008] Step S2. Cutting the first rolled slab into pieces and performing surface defect grinding treatment;

[0009] Step S3. The first rolled slab after the grinding treatment in step S2 is heated to T2 and kept at a temperature of t2, and then rolled in a hot rolling mill to a thickness of 4 mm to 8 mm to obtain a second rolled slab;

[0010] Step S4. performing surface defect grinding treatment on the second rolled slab;

[0011] Step S5. The second rolled slab after the surface defect grinding treatment in step S4 is heated to T3 and kept at temperature t3, and then rolled in a hot rolling mill to a thickness of 2.5 mm to 3.8 mm to obtain a third rolled slab;

[0012] Step S6. subjecting the third rolled slab to solution treatment and then cooling;

[0013] Step S7. sandblasting the third rolled slab after the solution treatment in step S6 to remove the oxide scale, then pickling, and then surface grinding;

[0014] Step S8. Sending the third rolled slab after surface grinding in step S7 to a cold rolling mill for cold rolling, and obtaining a cold rolled slab of target thickness after rolling;

[0015] Step S9. subjecting the cold-rolled slab to solution treatment and subsequent cooling;

[0016] Step S10. adding the cold-rolled slab after the solution treatment in step S9 to an alkali solution for alkali washing, and then adding the cold-rolled slab after the alkali washing to an acid washing solution for acid washing;

[0017] Step S11. Cut the slab after the pickling treatment in step S10 into fixed lengths to obtain titanium alloy sheets with a thickness of 0.6 mm to 1.5 mm.

[0018] Preferably, in the method for preparing the titanium alloy thin plate, T1 in step S1 is 1020°C to 1050°C, t1 is 120min to 192min, the single-pass deformation rate of the titanium alloy slab in the hot rolling mill is ≤20%, the rolling speed is ≥1.5m / s, and the final rolling temperature is controlled above the phase transformation point Tβ of the titanium alloy slab.

[0019] Preferably, in the method for preparing the titanium alloy thin plate, the grinding direction of the surface defect grinding treatment in step S2 is perpendicular to the rolling direction of the titanium alloy slab in step S1.

[0020] Preferably, the method for preparing the titanium alloy sheet is as follows, wherein T2 in step S3 is 880°C to 950°C, t2 is 10min to 20min, the single-pass deformation rate of the first rolled slab in the hot rolling mill is ≤25%, the rolling speed is ≥1.5m / s, the final rolling temperature is controlled above the phase transformation point Tβ of the titanium alloy slab, and the rolling direction is perpendicular to the rolling direction of the titanium alloy slab in step S1; and the grinding direction in step S4 is the same as the rolling direction of the first rolled slab in step S3.

[0021] Preferably, the method for preparing the titanium alloy thin plate, wherein in step S5, T3 is 880°C to 950°C, t3 is 4min to 8min, the single-pass deformation rate of the second rolled slab in the hot rolling mill is ≤35%, the rolling speed is ≥1.5m / s, the final rolling temperature is controlled above the phase transformation point Tβ of the titanium alloy slab, and the rolling direction is the same as the rolling direction of the first rolled slab in step S3.

[0022] Preferably, in the method for preparing the titanium alloy thin plate, the temperature of the solution treatment in step S6 is 800° C., the holding time is 10 to 25 minutes, and the cooling method is air cooling or wind cooling.

[0023] Preferably, in the method for preparing the titanium alloy thin plate, the thickness removal amount of the third rolled slab after sandblasting and pickling is controlled to be 0.06-0.10 mm in step S7.

[0024] Preferably, in the method for preparing the titanium alloy sheet, the cold rolling deformation in step S8 is controlled to be 45% to 75%.

[0025] Preferably, in the method for preparing the titanium alloy thin plate, the temperature of the solution treatment in step S9 is 760-820°C, and the holding time is 10-15 minutes; the cooling is specifically: the cold-rolled slab is air-cooled to below 200°C after being taken out of the furnace, and then air-cooled to room temperature.

[0026] Preferably, the method for preparing the titanium alloy thin plate, wherein, by mass percentage, the alkali solution in step S10 comprises 80% to 97% NaOH and 3% to 20% NaNO3, the alkali washing temperature is 460°C to 520°C, the alkali washing time is ≤5 min, the pickling solution comprises 1 to 5% HF, 30 to 40% HNO3 and 55 to 69% H2O, the pickling temperature is 10 to 45°C, the pickling time is ≤5 min, and the thickness removal amount of the cold-rolled slab treated by pickling is 0.06 mm to 0.10 mm.

[0027] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:

[0028] The preparation method of the titanium alloy thin plate of the present invention performs three-times hot rolling on the TB2 alloy slab, then performs solid solution treatment and surface descaling and contamination layer treatment on the slab, then rolls the slab to a desired thickness through 1 to 2 cold rolling processes, then performs solid solution treatment on the cold rolled slab, and finally obtains the TB2 titanium alloy thin plate that meets the requirements after surface treatment and finishing. The TB2 titanium alloy sheet material prepared by reasonably setting the hot and cold rolling deformation, heat treatment system and surface treatment process has good mechanical and process properties and meets the technical requirements of GB / T 3621, and can be mass-produced to produce TB2 titanium alloy thin plates that meet the performance requirements. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a metallographic test image of the titanium alloy thin plate prepared in Example 1 of the present invention.

[0030] Figure 2 This is a metallographic test image of the titanium alloy thin plate prepared in Example 2 of the present invention.

[0031] Figure 3 This is a metallographic test image of the titanium alloy thin plate prepared in Example 3 of the present invention. DETAILED DESCRIPTION

[0032] The present invention will be further described below in conjunction with specific embodiments.

[0033] Example 1

[0034] A method for preparing a titanium alloy thin plate comprises the following steps:

[0035] Step S1. A TB2 titanium alloy slab of 120×600×1000 mm is heated to 1050° C. in a box-type electric furnace and kept warm for 144 min, then taken out of the furnace and rolled on a hot rolling mill with a width of 1000 mm for eleven passes to a thickness of 15 mm to obtain a first rolled slab; the titanium alloy slab is rolled on the hot rolling mill for eleven passes with deformation rates of 10.8%, 14.0%, 15.2%, 16.7%, 18.5%, 18.9%, 18.6%, 20.0%, 17.9%, 19.5%, and 18.9% respectively, the rolling speed is 1.5 m / s, the phase transition point of the TB2 titanium alloy slab is 740° C., and the final rolling temperature is 920° C.;

[0036] Step S2. Cutting the first rolled slab into pieces of 1000 mm in length and grinding the surface defects, wherein the grinding direction of the surface defects is perpendicular to the rolling direction of the titanium alloy slab in step S1;

[0037] Step S3. The first rolled slab after the grinding treatment in step S2 is heated to 910°C in an electric furnace and kept warm for 15 minutes, then taken out of the furnace and rolled four times on a hot rolling mill to a thickness of 5.5 mm to obtain a second rolled slab; the deformation rates of the first rolled slab in the four rolling passes of the hot rolling mill are 20.0%, 25.0%, 22.2%, and 21.4% respectively, the rolling speed is 1.5 m / s, the final rolling temperature is 800°C, and the rolling direction is perpendicular to the rolling direction of the titanium alloy slab in step S1;

[0038] Step S4. Grinding the second rolled slab to remove surface defects, with the grinding direction being the same as the rolling direction of the first rolled slab in step S3;

[0039] Step S5. The second rolled slab after the surface defect grinding treatment in step S4 is heated to 910°C in an electric furnace and kept warm for 5 minutes, and then taken out of the furnace and rolled three times on a hot rolling mill to a thickness of 3.8 mm to obtain a third rolled slab; the second rolled slab is rolled three times on the hot rolling mill with deformation rates of 18.2%, 11.1%, and 5.0% respectively, the rolling speed is 1.5 m / s, the final rolling temperature is 750°C, and the rolling direction is the same as the rolling direction of the first rolled slab in step S3;

[0040] Step S6. subjecting the third rolled slab to a solution treatment in an electric heat treatment furnace at a temperature of 800°C for a holding time of 15 minutes, followed by air cooling;

[0041] Step S7. sandblasting the third rolled slab after the solution treatment in step S6 to remove the oxide scale, and then pickling, the pickling solution includes 3.5% HF, 30% HNO3 and 67.5% H2O by mass percentage, the pickling temperature is 32°C, the pickling time is 3 minutes, the thickness removal amount of the third rolled slab after sandblasting and pickling is controlled to be 0.08 mm, and then the surface is ground;

[0042] Step S8. Send the third rolled slab after surface grinding in step S7 to a cold rolling mill for cold rolling, and obtain a cold rolled slab with a thickness of 1.33 mm after rolling, and control the cold rolling deformation to be 65.0%;

[0043] Step S9. subjecting the cold-rolled slab to a solution treatment in an electric heat treatment furnace at a temperature of 780°C for a holding time of 10 minutes; subsequently, the cold-rolled slab is taken out of the furnace and air-cooled to below 200°C, and then air-cooled to room temperature;

[0044] Step S10. The cold-rolled slab after the solution treatment in step S9 is subjected to alkali washing treatment; the alkali solution is 88% NaOH + 12% NaNO3, the alkali washing temperature is 490°C, the alkali washing time is 3min, and then the cold-rolled slab after the alkali washing treatment is added to the pickling solution for pickling, the pickling solution includes 3.8% HF, 33% HNO3, 63.2% H2O, the pickling temperature is 35°C, the pickling time is 3 minutes and 30 seconds, and the thickness removal amount of the cold-rolled slab after the pickling treatment is 0.10mm;

[0045] Step S11. Cut the slab after the pickling treatment in step S10 into fixed lengths to obtain titanium alloy sheets with a size of 1.2×1000×2000 mm.

[0046] Example 2

[0047] A method for preparing a titanium alloy thin plate comprises the following steps:

[0048] Step S1. Heat a TB2 titanium alloy slab of 122×600×820 mm in a box-type electric furnace to 1050°C, keep it warm for 146 minutes, then take it out of the furnace and roll it on a hot rolling mill with a width of 820 mm for twelve passes to a thickness of 12 mm to obtain a first rolled slab; the deformation rates of the titanium alloy slab after twelve passes of rolling on the hot rolling mill are 12.3%, 14.0%, 15.2%, 16.7%, 18.5%, 18.9%, 18.6%, 20.0%, 17.9%, 19.5%, 18.9%, and 18.9% respectively, the rolling speed is 1.5 m / s, the phase change point is 740°C, and the final rolling temperature is 900°C.

[0049] Step S2. Cutting the first rolled slab into pieces of 1000 mm in length and grinding the surface defects, wherein the grinding direction of the surface defects is perpendicular to the rolling direction of the titanium alloy slab in step S1;

[0050] Step S3. The first rolled slab after the grinding treatment in step S2 is heated to 910°C in an electric furnace and kept at this temperature for 12 minutes, and then taken out of the furnace and rolled in a hot rolling mill for four passes to a thickness of 4.5 mm to obtain a second rolled slab;

[0051] The first rolled slab is rolled in four passes on a hot rolling mill with deformation rates of 12.5%, 23.8%, 25.0%, and 25.0% respectively, a rolling speed of 1.5 m / s, a final rolling temperature of 820° C., and a rolling direction perpendicular to the rolling direction of the titanium alloy slab in step S1;

[0052] Step S4. Grinding the second rolled slab to remove surface defects, with the grinding direction being the same as the rolling direction of the first rolled slab in step S3;

[0053] Step S5. The second rolled slab after the surface defect grinding treatment in step S4 is heated to 910° C. in an electric furnace and kept at this temperature for 4 minutes, and then taken out of the furnace and rolled three times in a hot rolling mill to a thickness of 2.8 mm to obtain a third rolled slab;

[0054] The second rolled slab is rolled in three passes in a hot rolling mill with deformation rates of 22.2%, 14.3%, and 6.7% respectively, a rolling speed of 1.5 m / s, a final rolling temperature of 750° C., and a rolling direction that is the same as that of the first rolled slab in step S3;

[0055] Step S6. subjecting the third rolled slab to a solution treatment in an electric heat treatment furnace at a temperature of 800°C for a holding time of 15 minutes, followed by air cooling;

[0056] Step S7. sandblasting the third rolled slab after the solution treatment in step S6 to remove the oxide scale, and then pickling, the pickling solution includes 2.9% HF, 33% HNO3, and 64.1% H2O by mass percentage, the pickling temperature is 30°C, the pickling time is 3 minutes and 40 seconds, and the thickness removal amount of the third rolled slab after sandblasting and pickling is controlled to be 0.08 mm, and then the surface is ground;

[0057] Step S8. Send the third rolled slab after surface grinding in step S7 to a cold rolling mill for cold rolling, and obtain a cold rolled slab with a thickness of 0.92 mm after rolling, and control the cold rolling deformation to be 67.1%;

[0058] Step S9. The cold-rolled slab is subjected to solution treatment in an electric heat treatment furnace, the temperature of the solution treatment is 780°C, and the holding time is 10 minutes; cooling is specifically: the cold-rolled slab is air-cooled to below 200°C after being taken out of the furnace, and then air-cooled to room temperature, and then cooled;

[0059] Step S10. Adding alkali solution to the cold-rolled slab after the solution treatment in step S9 for alkali washing; the alkali solution includes 91% NaOH and 9% NaNO3, the alkali washing temperature is 490°C, and the alkali washing time is 3 minutes. Then, the cold-rolled slab after the alkali washing is added to the pickling solution for pickling, the pickling solution includes 3.1% HF, 30% HNO3, and 66.9% H2O, the pickling temperature is 33°C, the pickling time is 3 minutes, and the thickness removal amount of the cold-rolled slab after the pickling treatment is 0.10 mm;

[0060] Step S11. Cut the slab after the pickling treatment in step S10 into a fixed length to obtain a titanium alloy sheet with a size of 0.8×1000×2000 mm.

[0061] Example 3

[0062] A method for preparing a titanium alloy thin plate comprises the following steps:

[0063] Step S1. Heating a TB2 titanium alloy slab of 140×590×825 mm in a box-type electric furnace to T1 and keeping the temperature at t1, then taking it out of the furnace and rolling it on a hot rolling mill for twelve passes to a thickness of 10 mm to obtain a first rolled slab; the titanium alloy slab is rolled on the hot rolling mill for twelve passes with deformation rates of 12.3%, 14.0%, 15.2%, 16.7%, 18.5%, 18.9%, 18.6%, 20.0%, 17.9%, 19.5%, 18.9%, 16.7% in sequence, the rolling speed is 1.5 m / s, the phase change point is 742°C, and the final rolling temperature is 910°C;

[0064] Step S2. Cutting the first rolled slab into pieces of 1000 mm in length and grinding the surface defects, wherein the grinding direction of the surface defects is perpendicular to the rolling direction of the titanium alloy slab in step S1;

[0065] Step S3. The first rolled slab after the grinding treatment in step S2 is heated to 910°C in an electric furnace and kept warm for 12 minutes, then taken out of the furnace and rolled four times on a hot rolling mill to a thickness of 4.2 mm to obtain a second rolled slab; the first rolled slab is rolled four times on the hot rolling mill with deformation rates of 20%, 25%, 16.7%, and 16% respectively, the rolling speed is 1.5 m / s, the final rolling temperature is 780°C, and the rolling direction is perpendicular to the rolling direction of the titanium alloy slab in step S1;

[0066] Step S4. Grinding the second rolled slab to remove surface defects, with the grinding direction being the same as the rolling direction of the first rolled slab in step S3;

[0067] Step S5. The second rolled slab after the surface defect grinding treatment in step S4 is heated to 910°C in an electric furnace and kept warm for 4 minutes, and then taken out of the furnace and rolled three times on a hot rolling mill to a thickness of 2.5 mm to obtain a third rolled slab; the second rolled slab is rolled three times on the hot rolling mill with deformation rates of 28.6%, 13.3%, and 4.0% respectively, the rolling speed is 1.5 m / s, the final rolling temperature is 760°C, and the rolling direction is the same as the rolling direction of the first rolled slab in step S3;

[0068] Step S6. subjecting the third rolled slab to a solution treatment in an electric heat treatment furnace at a temperature of 800°C for a holding time of 15 minutes, followed by air cooling;

[0069] Step S7. The third rolled slab after the solution treatment in step S6 is subjected to sandblasting to remove the oxide scale, and then pickled. The pickling solution includes 3.0% HF, 33% HNO3, and 64% H2O by mass percentage. The pickling temperature is 32° C. The pickling time is 3 minutes and 20 seconds. The thickness removal amount of the third rolled slab after sandblasting and pickling is controlled to be 0.08 mm, and then the surface is ground;

[0070] Step S8. Send the third rolled slab after surface grinding in step S7 to a cold rolling mill for cold rolling, and obtain a cold rolled slab with a thickness of 0.70 mm after rolling, and control the cold rolling deformation to be 72%;

[0071] Step S9. The cold-rolled slab is subjected to solution treatment in an electric heat treatment furnace, the temperature of the solution treatment is 780°C, and the holding time is 10 minutes; cooling is specifically: the cold-rolled slab is air-cooled to below 200°C after being taken out of the furnace, and then air-cooled to room temperature, and then cooled;

[0072] Step S10. Adding alkali solution to the cold-rolled slab after the solution treatment in step S9 for alkali washing; the alkali solution includes 87% NaOH and 13% NaNO3, the alkali washing temperature is 490°C, and the alkali washing time is 3 minutes. Then, the cold-rolled slab after the alkali washing is added to the pickling solution for pickling, the pickling solution includes 3.0% HF, 33% HNO3, and 64% H2O, the pickling temperature is 33°C, the pickling time is 3 minutes, and the thickness removal amount of the cold-rolled slab after the pickling treatment is 0.08 mm;

[0073] Step S11. Cut the slab after the pickling treatment in step S10 into fixed lengths to obtain titanium alloy thin plates with a size of 0.6×1000×2000 mm.

[0074] The performance test results of Examples 1, 2, and 3 are listed below. The results are shown in Table 1. From the results in Table 1, it can be concluded that the mechanical and process properties of the titanium alloy sheets prepared in Examples 1-3 meet the requirements of the standard GB / T3621 "Titanium and Titanium Alloy Sheets". The tensile strength, yield strength, elongation, and bending performance of sheets of different thicknesses are stable and have sufficient margins. The metallographic test results of Examples 1-3 are shown in Table 1. Figure 1-3 ,from Figure 1-3 It can be seen that the internal structure of the board is uniform and stable.

[0075] Table 1

[0076]

[0077] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.

Claims

1. A method for preparing a titanium alloy thin plate, characterized in that: The following steps are involved: Step S1. heating a titanium alloy slab with a thickness of 100 mm to 160 mm to T1 and keeping the temperature at t1, and then rolling it to a thickness of 10 mm to 20 mm in a hot rolling mill to obtain a first rolled slab; Step S2. Cutting the first rolled slab into pieces and performing surface defect grinding treatment; Step S3. The first rolled slab after the grinding treatment in step S2 is heated to T2 and kept at a temperature of t2, and then rolled in a hot rolling mill to a thickness of 4 mm to 8 mm to obtain a second rolled slab; Step S4. performing surface defect grinding treatment on the second rolled slab; Step S5. The second rolled slab after the surface defect grinding treatment in step S4 is heated to T3 and kept at temperature t3, and then rolled in a hot rolling mill to a thickness of 2.5 mm to 3.8 mm to obtain a third rolled slab; Step S6. subjecting the third rolled slab to solution treatment and then cooling; Step S7. sandblasting the third rolled slab after the solution treatment in step S6 to remove the oxide scale, then pickling, and then surface grinding; Step S8. Sending the third rolled slab after surface grinding in step S7 to a cold rolling mill for cold rolling, and obtaining a cold rolled slab of target thickness after rolling; Step S9. subjecting the cold-rolled slab to solution treatment and subsequent cooling; Step S10. adding the cold-rolled slab after the solution treatment in step S9 to an alkali solution for alkali washing, and then adding the cold-rolled slab after the alkali washing to an acid washing solution for acid washing; Step S11. Cut the slab after the pickling treatment in step S10 into a predetermined length to obtain a titanium alloy sheet with a thickness of 0.6 mm to 1.5 mm.

2. The method for preparing a titanium alloy sheet according to claim 1, characterized in that: In step S1, T1 is 1020°C to 1050°C, t1 is 120min to 192min, the single-pass deformation rate of the titanium alloy slab in the hot rolling mill is ≤20%, the rolling speed is ≥1.5m / s, and the final rolling temperature is controlled above the phase transformation point Tβ of the titanium alloy slab.

3. The method for preparing a titanium alloy sheet according to claim 1, characterized in that: The grinding direction of the surface defect grinding treatment in step S2 is perpendicular to the rolling direction of the titanium alloy slab in step S1.

4. The method for preparing a titanium alloy sheet according to claim 1, characterized in that: In step S3, T2 is 880℃~950℃, t2 is 10min~20min, the single-pass deformation rate of the first rolled slab in the hot rolling mill is ≤25%, the rolling speed is ≥1.5m / s, the final rolling temperature is controlled above the phase transformation point Tβ of the titanium alloy slab, and the rolling direction is perpendicular to the rolling direction of the titanium alloy slab in step S1; the grinding direction in step S4 is the same as the rolling direction of the first rolled slab in step S3.

5. The method for preparing a titanium alloy sheet according to claim 1, characterized in that: In step S5, T3 is 880℃~950℃, t3 is 4min~8min, the single-pass deformation rate of the second rolled slab in the hot rolling mill is ≤35%, the rolling speed is ≥1.5m / s, the final rolling temperature is controlled above the phase transformation point Tβ of the titanium alloy slab, and the rolling direction is the same as the rolling direction of the first rolled slab in step S3.

6. The method for preparing a titanium alloy sheet according to claim 1, characterized in that: The temperature of the solution treatment in step S6 is 800° C., the holding time is 10 to 25 minutes, and the cooling method is air cooling or wind cooling.

7. The method for preparing a titanium alloy sheet according to claim 1, characterized in that: In step S7, the thickness removal amount of the third rolled slab after sandblasting and pickling is controlled to be 0.06-0.10 mm.

8. The method for preparing a titanium alloy sheet according to claim 1, characterized in that: In step S8, the cold rolling deformation is controlled to be 45% to 75%.

9. The method for preparing a titanium alloy sheet according to claim 1, characterized in that: The temperature of the solution treatment in step S9 is 760-820°C, and the holding time is 10-15 minutes; the cooling is specifically as follows: the cold-rolled slab is air-cooled to below 200°C after being taken out of the furnace, and then air-cooled to room temperature.

10. The method for preparing a titanium alloy sheet according to claim 1, characterized in that: In terms of mass percentage, the alkali solution in step S10 includes 80% to 97% NaOH and 3% to 20% NaNO3, the alkali washing temperature is 460°C to 520°C, the alkali washing time is ≤5min, the pickling solution includes 1-5% HF, 30-40% HNO3 and 55-69% H2O, the pickling temperature is 10-45°C, the pickling time is ≤5min, and the thickness removal amount of the cold-rolled slab treated by pickling is 0.06mm to 0.10mm.

Citation Information

Patent Citations

  • Manufacturing method of TA6 titanium alloy large-width thin plate

    CN104439981A

  • Processing method of SP700 titanium alloy sheet for superplastic forming

    CN106955893A

  • Preparation method of TB8 titanium alloy sheet

    CN111054745A

  • Preparation method for TB5 alloy plate

    CN111471946A

  • Preparation method of titanium plate for deep drawing

    CN115961228A

Cited By

  • Metastable beta titanium alloy thin strip and preparation method thereof

    CN119870193A